Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.67 g/cm³ Show Material materials with Dichte of 2.67 g/cm³ | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.0 % Show Material materials with Dehnung of 14.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | F | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Härte, Brinell | 20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | EN 573-3 | Profile, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube | |
Schubmodule | 26.6 GPa Show Material materials with Schubmodule of 26.6 GPa | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 26.6 GPa Show Material materials with Schubmodule of 26.6 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
210.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 270.0 MPa | F | EN 573-3, EN 1715-3, EN 1715-4 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
215.0 - 385.0 MPa Show Material materials with Zugfestigkeit of 215.0 - 385.0 MPa | F | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | F | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | F | EN 573-3 | Flat | ||
20.0 °C | 215.0 MPa Show Material materials with Zugfestigkeit of 215.0 MPa | F | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium | ||||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | |
Wärmeleitfähigkeit | 20.0 °C | 129.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 129.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium | ||||
spezifischer Widerstand | 20.0 °C | 5.4e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.4e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | F | EN 573-3 | Profile, Rod, Flat, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Magnesium | 3.1 - 3.9 % Show Material materials with Magnesium of 3.1 - 3.9 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | F | EN 573-3, EN 1715-3, EN 1715-4, EN 485, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Welded Tube, Wire |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): sufficient - not suitable / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (O) |