Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.67 g/cm³ Show Material materials with Dichte of 2.67 g/cm³ | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
2.67 g/cm³ Show Material materials with Dichte of 2.67 g/cm³ | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H12 | EN 573-3 | Flat |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
Dehnung | 3.0 - 6.0 % Show Material materials with Dehnung of 3.0 - 6.0 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | A50 | |
3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | A50 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H12 | EN 573-3 | Flat | ||
Härte, Brinell | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | ||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H12 | EN 573-3 | Flat | ||
Härte, HBW | 75 [-] Show Material materials with Härte, HBW of 75 [-] | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H12 | EN 573-3 | Flat | |
Schubmodule | 25.725 GPa Show Material materials with Schubmodule of 25.725 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
26.6 GPa Show Material materials with Schubmodule of 26.6 GPa | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |||
20.0 °C | 26.6 GPa Show Material materials with Schubmodule of 26.6 GPa | H12 | EN 573-3 | Flat | ||
Streckgrenze | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | RP02 | |
190 MPa Show Material materials with Streckgrenze of 190 MPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |||
20.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H12 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Streckgrenze of 190.0 MPa | H12 | EN 573-3 | Flat | RP02 | |
Zugfestigkeit | 20.0 °C | 250.0 - 305.0 MPa Show Material materials with Zugfestigkeit of 250.0 - 305.0 MPa | H12 | EN 573-3 | Flat | Transverse |
20.0 °C | 250.0 - 305.0 MPa Show Material materials with Zugfestigkeit of 250.0 - 305.0 MPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3, EN 485 | Coil, Sheet, Strip, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | 20-100°C |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Spezifische Wärmekapazität | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H12 | EN 573-3 | Flat | |
Wärmeleitfähigkeit | 134 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 134 W/(m·K) | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
20.0 °C | 129.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 129.0 W/(m·K) | H12 | EN 573-3 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium | ||||
spezifischer Widerstand | 5.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.2e-08 Ω·m | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | ||
20.0 °C | 5.4e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.4e-08 Ω·m | H12 | EN 573-3 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.25 % Show Material materials with Chrom of 0.25 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H12 | EN 573-3 | Flat |
0.5 % Show Material materials with Eisen of 0.5 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
0.50 % Show Material materials with Eisen of 0.50 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.1 % Show Material materials with Kupfer of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Magnesium | 3.1 - 3.9 % Show Material materials with Magnesium of 3.1 - 3.9 % | H12 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 485 | Flat, Coil, Sheet, Strip, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.5 % Show Material materials with Mangan of 0.5 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.5 % Show Material materials with Silizium of 0.5 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.2 % Show Material materials with Titan of 0.2 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Rod, Welded Tube, Tube, Wire |
0.2 % Show Material materials with Zink of 0.2 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent | |
Application areas | Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Food can: Body, Lids | |
Brazing | hard brazing (with flux/ without flux): sufficient - not suitable / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Excellent | |
General machinability | Good | |
Welding | Good | |
Workability | Good |