Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.65 g/cm³ Show Material materials with Dichte of 2.65 g/cm³ | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | |
2.65 g/cm³ Show Material materials with Dichte of 2.65 g/cm³ | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | ||
20.0 °C | 2.64 g/cm³ Show Material materials with Dichte of 2.64 g/cm³ | H19 | EN 573-3 | Sheet, Flat |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | ||
71.0 GPa Show Material materials with Elastizitätsmodul of 71.0 GPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |||
Härte, Brinell | 114.0 [-] Show Material materials with Härte, Brinell of 114.0 [-] | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 114.0 [-] Show Material materials with Härte, Brinell of 114.0 [-] | H19 | EN 573-3 | Flat | ||
Härte, HBW | 114 [-] Show Material materials with Härte, HBW of 114 [-] | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 27.0 GPa Show Material materials with Schubmodule of 27.0 GPa | H19 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Coil, Sheet | |
Streckgrenze | 320.0 MPa Show Material materials with Streckgrenze of 320.0 MPa | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate | RP02 | |
320 MPa Show Material materials with Streckgrenze of 320 MPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |||
20.0 °C | 310.0 - 390.0 MPa Show Material materials with Streckgrenze of 310.0 - 390.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 310.0 - 340.0 MPa Show Material materials with Streckgrenze of 310.0 - 340.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
20.0 °C | 320.0 MPa Show Material materials with Streckgrenze of 320.0 MPa | H19 | EN 573-3 | Flat | RP02 | |
20.0 °C | 320.0 MPa Show Material materials with Streckgrenze of 320.0 MPa | H19 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 330.0 - 390.0 MPa Show Material materials with Streckgrenze of 330.0 - 390.0 MPa | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate | RP02 | |
20.0 °C | 330.0 - 340.0 MPa Show Material materials with Streckgrenze of 330.0 - 340.0 MPa | H19 | EN 573-3 | Sheet | RP02 | |
Zugfestigkeit | 380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | H19 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
380 MPa Show Material materials with Zugfestigkeit of 380 MPa | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |||
20.0 °C | 350.0 - 430.0 MPa Show Material materials with Zugfestigkeit of 350.0 - 430.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 350.0 - 390.0 MPa Show Material materials with Zugfestigkeit of 350.0 - 390.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 370.0 - 430.0 MPa Show Material materials with Zugfestigkeit of 370.0 - 430.0 MPa | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate | ||
20.0 °C | 370.0 - 390.0 MPa Show Material materials with Zugfestigkeit of 370.0 - 390.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | H19 | EN 573-3 | Flat | ||
20.0 °C | 380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | H19 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 577.0 - 638.0 °C Show Material materials with Schmelzpunkt of 577.0 - 638.0 °C | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | ||
Spezifische Wärmekapazität | 20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H19 | EN 573-3 | Sheet, Flat | |
Wärmeleitfähigkeit | 121 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121 W/(m·K) | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | ||
123 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 123 W/(m·K) | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | |||
20.0 °C | 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 W/(m·K) | H19 | EN 573-3 | Sheet, Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 S/m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | |
20.0 °C | 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 S/m | H19 | EN 573-3 | Sheet, Flat | |
spezifischer Widerstand | 5.56e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-08 Ω·m | H19 | EN 573-3, EN 485, EN 541 | Strip, Sheet, Plate | |
5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.6e-08 Ω·m | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Chrom of 0.1 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | H19 | EN 573-3 | Sheet, Flat |
0.35 % Show Material materials with Eisen of 0.35 % | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Coil, Sheet | |
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate |
0.15 % Show Material materials with Kupfer of 0.15 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |
Magnesium | 4.0 - 5.0 % Show Material materials with Magnesium of 4.0 - 5.0 % | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Strip, Plate, Coil, Sheet |
Mangan | 0.2 - 0.5 % Show Material materials with Mangan of 0.2 - 0.5 % | H19 | EN 573-3, EN 485, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Flat, Strip, Plate, Coil, Sheet |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate |
0.2 % Show Material materials with Silizium of 0.2 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Titan of 0.1 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H19 | EN 573-3, EN 485, EN 541 | Sheet, Flat, Strip, Plate |
0.25 % Show Material materials with Zink of 0.25 % | H19 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Application areas | Wind energy: Nacelle coverings, rotor hub, stairs; Components: Heat shields, Access hatches, Spoilers, General tranportation | |
Brazing | hard brazing (with flux/ without flux): sufficient to not suitable / poor, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Good | |
Workability | Bending / Spinning (cold): good / sufficient, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / acceptable (O) |