Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 14.0 % Show Material materials with Dehnung of 14.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | F | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Härte, Brinell | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | F | EN 573-3, EN 570 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | F | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube | |
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 26.3 - 26.5 GPa Show Material materials with Schubmodule of 26.3 - 26.5 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Zugfestigkeit | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
170.0 - 230.0 MPa Show Material materials with Zugfestigkeit of 170.0 - 230.0 MPa | F | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |||
20.0 °C | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | F | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 160.0 MPa Show Material materials with Zugfestigkeit of 160.0 MPa | F | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 650.0 °C Show Material materials with Schmelzpunkt of 610.0 - 650.0 °C | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 898.0 - 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 - 921.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 898.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Wärmeleitfähigkeit | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 149.0 - 167.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 149.0 - 167.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 149.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 149.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 25000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 25000000.0 - 30000000.0 S/m | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
20.0 °C | 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 26000000.0 S/m | F | EN 573-3 | Profile, Rod, Flat, Tube | |
spezifischer Widerstand | 3.33e-08 - 4e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 - 4e-08 Ω·m | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
20.0 °C | 4.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.15 % Show Material materials with Chrom of 0.15 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | F | EN 573-3 | Profile, Rod, Flat, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Magnesium | 1.7 - 2.4 % Show Material materials with Magnesium of 1.7 - 2.4 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Mangan | 0.1 - 0.5 % Show Material materials with Mangan of 0.1 - 0.5 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | F | EN 573-3, EN 1715-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12) |