Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H16 | EN 573-3 | Flat, Seamless Tube, Tube | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | H16 | EN 573-3 | Flat, Seamless Tube, Tube | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Plate, Strip, Flat, Seamless Tube, Tube |
Abmessung
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Dicke | 0.2 mm Show Material materials with Dicke of 0.2 mm | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | 0.2 mm | Coil, Sheet, Plate, Strip |
4.0 mm Show Material materials with Dicke of 4.0 mm | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | 4.0 mm | Coil, Sheet, Plate, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 3.5 °/t Show Material materials with Biegewinkel 180° of 3.5 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
3.5 °/t Show Material materials with Biegewinkel 180° of 3.5 °/t | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A50 | |
1.0 - 3.0 % Show Material materials with Dehnung of 1.0 - 3.0 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | H16 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H16 | EN 573-3, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A100 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H16 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H16 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H16 | EN 573-3 | Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H16 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H16 | EN 573-3 | Tube, Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H16 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H16 | EN 573-3 | Tube | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H16 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H16 | EN 573-3 | Seamless Tube | ||
Elastizitätsmodul | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
Härte, Brinell | 71.0 [-] Show Material materials with Härte, Brinell of 71.0 [-] | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | H16 | EN 573-3 | Tube | ||
20.0 °C | 71.0 [-] Show Material materials with Härte, Brinell of 71.0 [-] | H16 | EN 573-3 | Flat | ||
Härte, HBW | 71 [-] Show Material materials with Härte, HBW of 71 [-] | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H16 | EN 573-3 | Flat, Seamless Tube, Tube | |
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 26.3 - 26.5 GPa Show Material materials with Schubmodule of 26.3 - 26.5 GPa | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
20.0 °C | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
Streckgrenze | 180.0 MPa Show Material materials with Streckgrenze of 180.0 MPa | H16 | EN 573-3, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | RP02 | |
200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H16 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | RP02 | ||
200 MPa Show Material materials with Streckgrenze of 200 MPa | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |||
210.0 MPa Show Material materials with Streckgrenze of 210.0 MPa | H16 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 180.0 MPa Show Material materials with Streckgrenze of 180.0 MPa | H16 | EN 573-3 | Tube | RP02 | |
20.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H16 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 200.0 MPa Show Material materials with Streckgrenze of 200.0 MPa | H16 | EN 573-3 | Flat | RP02 | |
20.0 °C | 210.0 MPa Show Material materials with Streckgrenze of 210.0 MPa | H16 | EN 573-3 | Seamless Tube | RP02 | |
Zugfestigkeit | 245.0 MPa Show Material materials with Zugfestigkeit of 245.0 MPa | H16 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
20.0 °C | 220.0 - 260.0 MPa Show Material materials with Zugfestigkeit of 220.0 - 260.0 MPa | H16 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar | ||
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 270.0 MPa | H16 | EN 573-3 | Flat | Transverse | |
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 270.0 MPa | H16 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar, Coil, Sheet, Plate, Strip | ||
20.0 °C | 245.0 MPa Show Material materials with Zugfestigkeit of 245.0 MPa | H16 | EN 573-3 | Seamless Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 650.0 °C Show Material materials with Schmelzpunkt of 610.0 - 650.0 °C | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 898.0 - 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 - 921.0 J/(kg·K) | H16 | EN 573-3 | Flat, Seamless Tube, Tube | |
20.0 °C | 898.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 J/(kg·K) | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
Wärmeleitfähigkeit | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | ||
153 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 153 W/(m·K) | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |||
20.0 °C | 149.0 - 167.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 149.0 - 167.0 W/(m·K) | H16 | EN 573-3 | Flat, Seamless Tube, Tube | ||
20.0 °C | 149.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 149.0 W/(m·K) | H16 | EN 573-3 | Flat, Seamless Tube, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 25000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 25000000.0 - 30000000.0 S/m | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
20.0 °C | 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 26000000.0 S/m | H16 | EN 573-3 | Flat, Seamless Tube, Tube | |
spezifischer Widerstand | 3.33e-08 - 4e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 - 4e-08 Ω·m | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.5e-08 Ω·m | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | ||
20.0 °C | 4.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.6e-08 Ω·m | H16 | EN 573-3 | Flat, Seamless Tube, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip |
Chrom | 0.15 % Show Material materials with Chrom of 0.15 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
0.15 % Show Material materials with Chrom of 0.15 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H16 | EN 573-3 | Flat, Seamless Tube, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Strip, Sheet, Plate, Wire, Tube, Welded Tube, Bar | |
0.5 % Show Material materials with Eisen of 0.5 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
0.15 % Show Material materials with Kupfer of 0.15 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |
Magnesium | 1.7 - 2.4 % Show Material materials with Magnesium of 1.7 - 2.4 % | H16 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar, Coil, Sheet, Plate, Strip |
Mangan | 0.1 - 0.5 % Show Material materials with Mangan of 0.1 - 0.5 % | H16 | EN 573-3, EN 1592, EN 485, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar, Coil, Sheet, Plate, Strip |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
0.4 % Show Material materials with Silizium of 0.4 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
0.15 % Show Material materials with Titan of 0.15 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip | |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | H16 | EN 573-3, EN 1592, EN 485, EN 754 | Flat, Seamless Tube, Tube, Strip, Sheet, Plate, Wire, Welded Tube, Bar |
0.15 % Show Material materials with Zink of 0.15 % | H16 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Tubes: Industrial tubes, Pipes; Wind energy: Nacelle coverings, rotor hub, stairs; | |
Brazing | hard brazing (with flux/ without flux): sufficient / poor, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / acceptable (H12) |