Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
1.5 °/t Show Material materials with Biegewinkel 180° of 1.5 °/t | H111 | EN 573-3, EN 14286, EN 485 | Strip, Sheet, Plate | |||
4.0 °/t Show Material materials with Biegewinkel 180° of 4.0 °/t | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Dehnung | 11.0 % Show Material materials with Dehnung of 11.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | |||
17.0 % Show Material materials with Dehnung of 17.0 % | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | A100 | ||
20.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Sheet | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Sheet | ||
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Härte, Brinell | 70.0 [-] Show Material materials with Härte, Brinell of 70.0 [-] | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | ||
75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
76.0 [-] Show Material materials with Härte, Brinell of 76.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
85.0 [-] Show Material materials with Härte, Brinell of 85.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 75.0 - 85.0 [-] Show Material materials with Härte, Brinell of 75.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 75.0 - 80.0 [-] Show Material materials with Härte, Brinell of 75.0 - 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 75.0 - 76.0 [-] Show Material materials with Härte, Brinell of 75.0 - 76.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 76.0 - 85.0 [-] Show Material materials with Härte, Brinell of 76.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 76.0 - 80.0 [-] Show Material materials with Härte, Brinell of 76.0 - 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 76.0 [-] Show Material materials with Härte, Brinell of 76.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 80.0 - 85.0 [-] Show Material materials with Härte, Brinell of 80.0 - 85.0 [-] | H111 | EN 573-3 | Flat | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | H111 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 85.0 [-] Show Material materials with Härte, Brinell of 85.0 [-] | H111 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 75.0 - 80.0 MPa Show Material materials with Scherfestigkeit of 75.0 - 80.0 MPa | H111 | EN 573-3 | Sheet | |
20.0 °C | 75.0 - 76.0 MPa Show Material materials with Scherfestigkeit of 75.0 - 76.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 75.0 MPa Show Material materials with Scherfestigkeit of 75.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 76.0 - 80.0 MPa Show Material materials with Scherfestigkeit of 76.0 - 80.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 76.0 MPa Show Material materials with Scherfestigkeit of 76.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 80.0 MPa Show Material materials with Scherfestigkeit of 80.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 85.0 MPa Show Material materials with Scherfestigkeit of 85.0 MPa | H111 | EN 573-3 | Flat | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Zugfestigkeit | 270.0 MPa Show Material materials with Zugfestigkeit of 270.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
275.0 MPa Show Material materials with Zugfestigkeit of 275.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | H111 | EN 573-3, EN 13195 | Strip, Sheet, Plate | |||
290.0 - 370.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 370.0 MPa | H111 | EN 573-3, EN 14286 | Strip, Sheet, Plate | |||
20.0 °C | 270.0 - 360.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 270.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 270.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 355.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 275.0 - 360.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 275.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 275.0 - 355.0 MPa | H111 | EN 573-3 | Sheet | ||
20.0 °C | 285.0 - 360.0 MPa Show Material materials with Zugfestigkeit of 285.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 285.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 285.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 285.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 285.0 - 355.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 290.0 - 360.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 360.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 290.0 - 355.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 355.0 MPa | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 290.0 - 360.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 360.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 205.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Eisen | 0.25 % Show Material materials with Eisen of 0.25 % | H111 | EN 573-3 | Flat, Sheet |
0.25 % Show Material materials with Eisen of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Strip, Sheet, Plate | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Magnesium | 4.0 - 5.2 % Show Material materials with Magnesium of 4.0 - 5.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Mangan | 0.7 - 1.0 % Show Material materials with Mangan of 0.7 - 1.0 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Zink | 0.4 % Show Material materials with Zink of 0.4 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Zirkonium | 0.2 % Show Material materials with Zirkonium of 0.2 % | H111 | EN 573-3, EN 13195, EN 14286, EN 485 | Flat, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |