Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
3.0 °/t Show Material materials with Biegewinkel 180° of 3.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
3.5 °/t Show Material materials with Biegewinkel 90° of 3.5 °/t | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
Dehnung | 5.0 % Show Material materials with Dehnung of 5.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | |
6.0 % Show Material materials with Dehnung of 6.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H22 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H22 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H22 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | H22 | EN 573-3 | Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H22 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H22 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H22 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H22 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Härte, Brinell | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | H22 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Scherfestigkeit | 20.0 °C | 90.0 MPa Show Material materials with Scherfestigkeit of 90.0 MPa | H22 | EN 573-3 | Flat | |
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 305.0 - 380.0 MPa Show Material materials with Zugfestigkeit of 305.0 - 380.0 MPa | H22 | EN 573-3 | Flat | Transverse |
20.0 °C | 305.0 - 380.0 MPa Show Material materials with Zugfestigkeit of 305.0 - 380.0 MPa | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate, Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 205.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.25 % Show Material materials with Chrom of 0.25 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Eisen | 0.25 % Show Material materials with Eisen of 0.25 % | H22 | EN 573-3 | Flat |
0.25 % Show Material materials with Eisen of 0.25 % | H22 | EN 573-3, EN 485 | Strip, Sheet, Plate | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Magnesium | 4.0 - 5.2 % Show Material materials with Magnesium of 4.0 - 5.2 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Mangan | 0.7 - 1.0 % Show Material materials with Mangan of 0.7 - 1.0 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Zink | 0.4 % Show Material materials with Zink of 0.4 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Zirkonium | 0.2 % Show Material materials with Zirkonium of 0.2 % | H22 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |