Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H28 | EN 573-3 | Flat, Seamless Tube | |
20.0 °C | 2.68 - 2.69 g/cm³ Show Material materials with Dichte of 2.68 - 2.69 g/cm³ | H28 | EN 573-3 | Flat, Seamless Tube | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 573-3 | Coil, Sheet, Plate, Flat, Seamless Tube |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 145.0 MPa Show Material materials with Bending Fatigue Strength of 145.0 MPa | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | |
3 % Show Material materials with Dehnung of 3 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H28 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H28 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H28 | EN 573-3 | Seamless Tube | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H28 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | ||
70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H28 | EN 573-3 | Flat, Seamless Tube | ||
Härte, Brinell | 93.0 [-] Show Material materials with Härte, Brinell of 93.0 [-] | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 93.0 [-] Show Material materials with Härte, Brinell of 93.0 [-] | H28 | EN 573-3 | Flat | ||
Härte, HBW | 93 [-] Show Material materials with Härte, HBW of 93 [-] | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H28 | EN 573-3 | Flat, Seamless Tube | |
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
26.6 GPa Show Material materials with Schubmodule of 26.6 GPa | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Schubmodule of 26.5 - 27.0 GPa | H28 | EN 573-3 | Flat, Seamless Tube | ||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H28 | EN 573-3 | Flat, Seamless Tube | ||
Streckgrenze | 250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | RP02 | |
250 MPa Show Material materials with Streckgrenze of 250 MPa | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
280.0 MPa Show Material materials with Streckgrenze of 280.0 MPa | H28 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Rod, Tube | RP02 | ||
20.0 °C | 250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | H28 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 250.0 MPa Show Material materials with Streckgrenze of 250.0 MPa | H28 | EN 573-3 | Flat | RP02 | |
20.0 °C | 280.0 MPa Show Material materials with Streckgrenze of 280.0 MPa | H28 | EN 573-3 | Seamless Tube | RP02 | |
Zugfestigkeit | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
310 MPa Show Material materials with Zugfestigkeit of 310 MPa | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | H28 | EN 573-3 | Flat | Transverse | |
20.0 °C | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | H28 | EN 573-3 | Seamless Tube, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1899999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1899999999999997e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
-50.0 °C | 2.19e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.19e-05 1/K | H28 | EN 573-3 | Flat, Seamless Tube | ||
20 °C | 2.1899999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1899999999999997e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
20 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
100.0 °C | 2.37e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.37e-05 1/K | H28 | EN 573-3 | Flat, Seamless Tube | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | 20-100°C | |
200 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
200.0 °C | 2.46e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.46e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
300 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
300.0 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat, Seamless Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 602.0 - 646.0 °C Show Material materials with Schmelzpunkt of 602.0 - 646.0 °C | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 897.0 - 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 - 900.0 J/(kg·K) | H28 | EN 573-3 | Flat, Seamless Tube | ||
20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H28 | EN 573-3 | Flat, Seamless Tube | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H28 | EN 573-3 | Flat, Seamless Tube | ||
Wärmeleitfähigkeit | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
134 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 134 W/(m·K) | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |||
20.0 °C | 135.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 135.0 - 150.0 W/(m·K) | H28 | EN 573-3 | Flat, Seamless Tube | ||
20.0 °C | 135.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 135.0 W/(m·K) | H28 | EN 573-3 | Flat, Seamless Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 S/m | H28 | EN 573-3 | Flat, Seamless Tube | |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 5.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.1e-08 Ω·m | H28 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Coil, Sheet, Plate |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Andere | 0.05 - 0.15 % Show Material materials with Andere of 0.05 - 0.15 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Chrom | 0.05 - 0.2 % Show Material materials with Chrom of 0.05 - 0.2 % | H28 | EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube, Coil, Sheet, Plate |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H28 | EN 573-3 | Flat, Seamless Tube |
0.40 % Show Material materials with Eisen of 0.40 % | H28 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
0.4 % Show Material materials with Eisen of 0.4 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H28 | EN 573-3, EN 1592, EN 485 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube |
0.1 % Show Material materials with Kupfer of 0.1 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Magnesium | 2.4 - 3.0 % Show Material materials with Magnesium of 2.4 - 3.0 % | H28 | EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube, Coil, Sheet, Plate |
Mangan | 0.5 - 1.0 % Show Material materials with Mangan of 0.5 - 1.0 % | H28 | EN 573-3, EN 1592, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube, Coil, Sheet, Plate |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H28 | EN 573-3, EN 1592, EN 485 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube |
0.25 % Show Material materials with Silizium of 0.25 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | H28 | EN 573-3, EN 1592, EN 485 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube |
0.2 % Show Material materials with Titan of 0.2 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H28 | EN 573-3, EN 1592, EN 485 | Flat, Seamless Tube, Strip, Sheet, Plate, Rod, Tube |
0.25 % Show Material materials with Zink of 0.25 % | H28 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet, Plate |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Application areas | Vessels: Pressure; Components: General transportation | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
General machinability | Fair | |
Surface Finish | Mill finish. | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |