Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 2.66 - 2.68 g/cm³ Show Material materials with Dichte of 2.66 - 2.68 g/cm³ | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | H12 | EN 573-3 | Wire, Flat, Seamless Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A100 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | A50 | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3 | Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3 | Seamless Tube, Flat | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 70.0 - 70.5 GPa Show Material materials with Elastizitätsmodul of 70.0 - 70.5 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 70.5 GPa Show Material materials with Elastizitätsmodul of 70.5 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
Härte, Brinell | 66.0 [-] Show Material materials with Härte, Brinell of 66.0 [-] | H12 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 66.0 [-] Show Material materials with Härte, Brinell of 66.0 [-] | H12 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 26.5 - 27.0 GPa Show Material materials with Schubmodule of 26.5 - 27.0 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H12 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | H12 | EN 573-3 | Seamless Tube | ||
20.0 °C | 220.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 220.0 - 270.0 MPa | H12 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
20.0 °C | 220.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 220.0 - 270.0 MPa | H12 | EN 573-3 | Flat | Transverse | |
20.0 °C | 230.0 - 280.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 280.0 MPa | H12 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Forging, Tube, Bar |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
100.0 °C | 2.39e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.39e-05 1/K | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 610.0 - 640.0 °C Show Material materials with Schmelzpunkt of 610.0 - 640.0 °C | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 897.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 - 963.0 J/(kg·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
Wärmeleitfähigkeit | 20.0 °C | 132.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 - 160.0 W/(m·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 132.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 - 140.0 W/(m·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 132.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 132.0 W/(m·K) | H12 | EN 573-3 | Wire, Flat, Seamless Tube | ||
20.0 °C | 140.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 160.0 W/(m·K) | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Seamless Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 23000000.0 S/m | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar, Flat, Seamless Tube |
spezifischer Widerstand | 4.35e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5e-08 Ω·m | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
20.0 °C | 4.3e-08 - 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-08 - 5.3e-08 Ω·m | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 4.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.3e-08 - 5e-08 Ω·m | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 5e-08 - 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 5e-08 - 5.3e-08 Ω·m | H12 | EN 573-3 | Wire, Flat, Seamless Tube | |
20.0 °C | 5.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.3e-08 Ω·m | H12 | EN 573-3 | Wire, Flat, Seamless Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H12 | EN 573-3 | Wire, Flat, Seamless Tube |
0.40 % Show Material materials with Eisen of 0.40 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Strip, Sheet, Plate, Wire, Forging, Tube, Bar | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Magnesium | 2.6 - 3.6 % Show Material materials with Magnesium of 2.6 - 3.6 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H12 | EN 573-3, EN 1301, EN 1592, EN 485 | Wire, Flat, Seamless Tube, Strip, Sheet, Plate, Forging, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good to good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |