Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | Typical for Wrought 6000 Series Aluminium |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | Typical for Wrought 6000 Series Aluminium | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||
Zugfestigkeit | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6 | AA Standards, ASTM B221 | |
290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B483 |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 6000 Series Aluminium |
Schmelzpunkt | 555.0 - 655.0 °C Show Material materials with Schmelzpunkt of 555.0 - 655.0 °C | Typical for Wrought 6000 Series Aluminium |
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium |
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | Typical for Wrought 6000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 21000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 21000000.0 - 34000000.0 S/m | Typical for Wrought 6000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5e-08 Ω·m | Typical for Wrought 6000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Bismut | 0.4 - 0.7 % Show Material materials with Bismut of 0.4 - 0.7 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Blei | 0.4 - 0.7 % Show Material materials with Blei of 0.4 - 0.7 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Chrom | 0.04 - 0.14 % Show Material materials with Chrom of 0.04 - 0.14 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Kupfer | 0.15 - 0.4 % Show Material materials with Kupfer of 0.15 - 0.4 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | T6 | AA Standards, ASTM B210, ASTM B211, ASTM B221, ASTM B483 |
Technological properties
Property | ||
---|---|---|
Brazing | general: Lötbar mit speziellen Techniken oder bei bestimmten Anwendungen | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: good, without protection in industrial or seawater atmosphere | |
General machinability | General: good to acceptable (T6, T651, T6510, T6511, T9) | |
Workability | general (condition): poor(T6, T651, T6510, T6511), not suitable (T9) |