Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T6510 | EN 573-3, EN 755 | Rod, Tube | |
20.0 °C | 2.75 g/cm³ Show Material materials with Dichte of 2.75 g/cm³ | T6510 | EN 573-3 | Profile, Rod, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A50 | |
8.0 % Show Material materials with Dehnung of 8.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A100 | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T6510 | EN 573-3 | Profile, Tube, Rod | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
Härte, Brinell | 20.0 °C | 105.0 [-] Show Material materials with Härte, Brinell of 105.0 [-] | T6510 | EN 573-3 | Profile, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | ||||
Zugfestigkeit | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
20.0 °C | 260.0 MPa Show Material materials with Zugfestigkeit of 260.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T6510 | EN 573-3 | Profile, Tube, Rod |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T6510 | EN 573-3, EN 755 | Rod, Tube | |
100.0 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | T6510 | EN 573-3 | Profile, Rod, Tube | ||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
Schmelzpunkt | 585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
20.0 °C | 163.0 - 186.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 163.0 - 186.0 W/(m·K) | T6510 | EN 573-3 | Profile, Rod, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 32000000.0 S/m | T6510 | EN 573-3, EN 755 | Rod, Tube | |
20.0 °C | 24000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 28000000.0 S/m | T6510 | EN 573-3 | Profile, Rod, Tube | |
spezifischer Widerstand | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-08 - 4.17e-08 Ω·m | T6510 | EN 573-3, EN 755 | Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismut | 0.7 % Show Material materials with Bismut of 0.7 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Blei | 0.4 - 2.0 % Show Material materials with Blei of 0.4 - 2.0 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | T6510 | EN 573-3 | Profile, Rod, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | T6510 | EN 573-3, EN 755 | Rod, Tube | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Magnesium | 0.6 - 1.2 % Show Material materials with Magnesium of 0.6 - 1.2 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Mangan | 0.4 - 1.0 % Show Material materials with Mangan of 0.4 - 1.0 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Silizium | 0.6 - 1.4 % Show Material materials with Silizium of 0.6 - 1.4 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Zink | 0.3 % Show Material materials with Zink of 0.3 % | T6510 | EN 573-3, EN 755 | Profile, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | Protective: acceptable | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable | |
Corrosion properties | Seawater: acceptable, weathering: good | |