Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.71 - 2.72 g/cm³ Show Material materials with Dichte of 2.71 - 2.72 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | F | EN 573-3 | Profile, Rod, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 18.0 % Show Material materials with Dehnung of 18.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
20.0 % Show Material materials with Dehnung of 20.0 % | F | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | F | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | F | EN 573-3 | Profile, Rod, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 60.0 - 65.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 65.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 65.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 65.0 - 69.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Härte, Brinell | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | F | EN 573-3, EN 570 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 23.0 [-] Show Material materials with Härte, Brinell of 23.0 [-] | F | EN 573-3 | Profile, Rod, Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | F | EN 573-3 | Profile, Rod, Flat, Tube | |
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 24.0 - 26.0 GPa Show Material materials with Schubmodule of 24.0 - 26.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 24.0 - 25.9 GPa Show Material materials with Schubmodule of 24.0 - 25.9 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 25.9 - 26.0 GPa Show Material materials with Schubmodule of 25.9 - 26.0 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
20.0 °C | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | F | EN 573-3 | Profile, Rod, Flat, Tube | ||
Zugfestigkeit | 75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | F | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | F | EN 573-3 | Profile, Rod, Tube, Flat | ||
20.0 °C | 75.0 MPa Show Material materials with Zugfestigkeit of 75.0 MPa | F | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat |
-50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | F | EN 573-3 | Profile, Rod, Flat, Tube | |
Schmelzpunkt | 644.0 - 657.0 °C Show Material materials with Schmelzpunkt of 644.0 - 657.0 °C | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Spezifische Wärmekapazität | 20.0 °C | 898.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 J/(kg·K) | F | EN 573-3 | Profile, Rod, Flat, Tube |
Wärmeleitfähigkeit | 20.0 °C | 205.0 - 210.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 205.0 - 210.0 W/(m·K) | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Profile, Flat |
20.0 °C | 205.0 - 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 205.0 - 225.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 210.0 - 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 225.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube | |
20.0 °C | 225.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 225.0 W/(m·K) | F | EN 573-3 | Profile, Rod, Flat, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 34000000.0 S/m | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34400000.0 - 35500000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34400000.0 - 35500000.0 S/m | F | EN 573-3 | Profile, Rod, Flat, Tube | |
spezifischer Widerstand | 2.94e-08 - 3.03e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.03e-08 Ω·m | F | EN 573-3, EN 485, EN 570, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.95e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.95e-08 Ω·m | F | EN 573-3 | Profile, Rod, Flat, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | F | EN 573-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | F | EN 573-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | F | EN 573-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | F | EN 573-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | F | EN 573-3, EN 485, EN 570, EN 755 | Profile, Rod, Flat, Tube, Strip, Sheet, Plate, Foil, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H12) / very good (H12) |