Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 25.0 MPa Show Material materials with Bending Fatigue Strength of 25.0 MPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
35.0 MPa Show Material materials with Bending Fatigue Strength of 35.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Biegewinkel 180° | 1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3, EN 485, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Foil, Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Rod, Tube, Flat | ||
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
-195.0 °C | 78.4 GPa Show Material materials with Elastizitätsmodul of 78.4 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
-85.0 °C | 73.5 GPa Show Material materials with Elastizitätsmodul of 73.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
-30.0 °C | 71.4 GPa Show Material materials with Elastizitätsmodul of 71.4 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 - 68.6 GPa Show Material materials with Elastizitätsmodul of 68.0 - 68.6 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 - 66.5 GPa Show Material materials with Elastizitätsmodul of 66.0 - 66.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.5 GPa Show Material materials with Elastizitätsmodul of 66.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 56.0 - 57.0 GPa Show Material materials with Elastizitätsmodul of 56.0 - 57.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 56.0 GPa Show Material materials with Elastizitätsmodul of 56.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Härte, Brinell | 34.0 [-] Show Material materials with Härte, Brinell of 34.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 30.0 [-] Show Material materials with Härte, Brinell of 30.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 34.0 [-] Show Material materials with Härte, Brinell of 34.0 [-] | H14 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Schubmodule of 25.0 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.0 - 25.9 GPa Show Material materials with Schubmodule of 25.0 - 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.9 - 26.5 GPa Show Material materials with Schubmodule of 25.9 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Zugfestigkeit | 100.0 MPa Show Material materials with Zugfestigkeit of 100.0 MPa | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 100.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 135.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 100.0 MPa Show Material materials with Zugfestigkeit of 100.0 MPa | H14 | EN 573-3 | Wire | ||
20.0 °C | 105.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 145.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 105.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 145.0 MPa | H14 | EN 573-3, EN 485, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
-50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Schmelzpunkt | 646.0 - 657.0 °C Show Material materials with Schmelzpunkt of 646.0 - 657.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 899.0 - 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 - 900.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
20.0 °C | 210.0 - 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 220.0 - 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 220.0 - 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 229.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 34000000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 36000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34800000.0 - 36000000.0 S/m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
spezifischer Widerstand | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.94e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.8e-08 - 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.8e-08 - 2.9e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Bor | 0.05 Show Material materials with Bor of 0.05 | H14 | EN 573-3 | Flat |
Chrom | 0.01 Show Material materials with Chrom of 0.01 | H14 | EN 573-3 | Flat |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | H14 | EN 573-3 | Flat, Rod, Foil, Tube, Wire |
0.40 % Show Material materials with Eisen of 0.40 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Gallium | 0.03 Show Material materials with Gallium of 0.03 | H14 | EN 573-3 | Flat |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Magnesium | 0.03 % Show Material materials with Magnesium of 0.03 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Magnesium of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Mangan of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Nickel | 0.03 Show Material materials with Nickel of 0.03 | H14 | EN 573-3 | Flat |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | H14 | EN 573-3 | Flat |
0.25 % Show Material materials with Silizium of 0.25 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | H14 | EN 573-3 | Flat |
0.05 % Show Material materials with Titan of 0.05 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar | |
Vanadium | 0.03 Show Material materials with Vanadium of 0.03 | H14 | EN 573-3 | Flat |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | H14 | EN 573-3 | Flat |
0.07 % Show Material materials with Zink of 0.07 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Flat, Rod, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |