Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | T4 | EN 573-3 | Profile, Rod, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A50 | |
12.0 % Show Material materials with Dehnung of 12.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |||
14.0 % Show Material materials with Dehnung of 14.0 % | T4 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | T4 | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |||
15.0 % Show Material materials with Dehnung of 15.0 % | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | T4 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | T4 | EN 573-3 | Tube | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | T4 | EN 573-3 | Tube | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | T4 | EN 573-3 | Wire | A100 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | T4 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | T4 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | T4 | EN 573-3 | Rod, Tube, Profile | ||
Elastizitätsmodul | -270 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T4 | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |
-196.0 °C | 65.0 GPa Show Material materials with Elastizitätsmodul of 65.0 GPa | T4 | EN 573-3 | |||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | T4 | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | |||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 65.0 GPa Show Material materials with Elastizitätsmodul of 65.0 GPa | T4 | EN 573-3 | |||
20.0 °C | 67.0 GPa Show Material materials with Elastizitätsmodul of 67.0 GPa | T4 | EN 573-3 | Profile, Rod, Tube, Wire | ||
20 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T4 | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | ||
50.0 °C | 65.0 GPa Show Material materials with Elastizitätsmodul of 65.0 GPa | T4 | EN 573-3 | |||
300 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | T4 | EN 573-3 | Strip, Sheet, Plate, Tube, Bar | ||
Härte, Brinell | 20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | T4 | EN 573-3 | Profile, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | T4 | EN 573-3 | Profile, Rod, Tube, Wire | ||
Zugfestigkeit | 120.0 MPa Show Material materials with Zugfestigkeit of 120.0 MPa | T4 | EN 573-3, EN 12020, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | T4 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | |||
140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | T4 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |||
155.0 - 210.0 MPa Show Material materials with Zugfestigkeit of 155.0 - 210.0 MPa | T4 | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 120.0 MPa Show Material materials with Zugfestigkeit of 120.0 MPa | T4 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | T4 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 140.0 - 210.0 MPa Show Material materials with Zugfestigkeit of 140.0 - 210.0 MPa | T4 | EN 573-3 | Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
20 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
200 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
300 °C | 2.56e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.56e-05 1/K | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Schmelzpunkt | 585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Spezifische Wärmekapazität | 898.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 898.0 J/(kg·K) | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Wärmeleitfähigkeit | 200.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200.0 - 220.0 W/(m·K) | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 220.0 W/(m·K) | T4 | EN 573-3 | Profile, Rod, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 28000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 28000000.0 - 31000000.0 S/m | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 30000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 30000000.0 - 32000000.0 S/m | T4 | EN 573-3 | Profile, Rod, Tube, Wire | |
spezifischer Widerstand | 3.23e-08 - 3.57e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.23e-08 - 3.57e-08 Ω·m | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 % Show Material materials with Chrom of 0.05 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Eisen | 0.1 - 0.3 % Show Material materials with Eisen of 0.1 - 0.3 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Magnesium | 0.35 - 0.6 % Show Material materials with Magnesium of 0.35 - 0.6 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Silizium | 0.3 - 0.6 % Show Material materials with Silizium of 0.3 - 0.6 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | T4 | EN 573-3, EN 12020, EN 1301, EN 1715-3, EN 754, EN 755 | Profile, Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: EQ: sehr gut, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / good, friction soldering: very good, soft brazing with flux: good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / -, Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) - / good (O) |