Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 68.3 - 69.6 GPa Show Material materials with Elastizitätsmodul of 68.3 - 69.6 GPa | H18 | EN 573-3 | Wire | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.3 GPa Show Material materials with Schubmodule of 26.3 GPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 26.2 GPa Show Material materials with Schubmodule of 26.2 GPa | H18 | EN 573-3 | Wire | ||
Zugfestigkeit | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H18 | EN 573-3 | Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar |
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.3e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Schmelzpunkt | 580.0 - 640.0 °C Show Material materials with Schmelzpunkt of 580.0 - 640.0 °C | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
580.0 - 650.0 °C Show Material materials with Schmelzpunkt of 580.0 - 650.0 °C | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 870.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 870.0 J/(kg·K) | H18 | EN 573-3 | Wire |
Wärmeleitfähigkeit | 155.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 155.0 - 180.0 W/(m·K) | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
170.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 200.0 W/(m·K) | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 150.0 - 165.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 150.0 - 165.0 W/(m·K) | H18 | EN 573-3 | Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 22000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 30000000.0 S/m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
23000000.0 - 27000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 27000000.0 S/m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 20000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 30000000.0 S/m | H18 | EN 573-3 | Wire | |
spezifischer Widerstand | 3.33e-08 - 4.55e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 - 4.55e-08 Ω·m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
3.7e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.7e-08 - 4.35e-08 Ω·m | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.04 - 0.35 % Show Material materials with Chrom of 0.04 - 0.35 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H18 | EN 573-3 | Wire |
0.70 % Show Material materials with Eisen of 0.70 % | H18 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Kupfer | 0.15 - 0.4 % Show Material materials with Kupfer of 0.15 - 0.4 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Magnesium | 0.8 - 1.2 % Show Material materials with Magnesium of 0.8 - 1.2 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H18 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): good / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Bending / Spinning (cold): acceptable (T3, T4) / good (O), Impact extrusion (cold): good (O), Deep drawing / upsetting (Condition) good (O) / good (O) |