Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A50 | |
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Tube | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 18.0 % Show Material materials with Dehnung of 18.0 % | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H111 | EN 573-3 | Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |||
Härte, Brinell | 20.0 °C | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | H111 | EN 573-3 | Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | ||||
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Zugfestigkeit | 130.0 Show Material materials with Zugfestigkeit of 130.0 | H111 | EN 573-3, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
155.0 Show Material materials with Zugfestigkeit of 155.0 | H111 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | |||
20.0 °C | 130.0 Show Material materials with Zugfestigkeit of 130.0 | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 140.0 Show Material materials with Zugfestigkeit of 140.0 | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 150.0 Show Material materials with Zugfestigkeit of 150.0 | H111 | EN 573-3 | Rod, Tube | ||
20.0 °C | 155.0 Show Material materials with Zugfestigkeit of 155.0 | H111 | EN 573-3 | Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Schmelzpunkt | 615.0 - 655.0 °C Show Material materials with Schmelzpunkt of 615.0 - 655.0 °C | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Wärmeleitfähigkeit | 193.0 - 218.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193.0 - 218.0 W/(m·K) | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 - 34000000.0 S/m | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
spezifischer Widerstand | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.45e-08 Ω·m | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 % Show Material materials with Chrom of 0.05 % | H111 | EN 573-3 | Rod, Tube |
0.1 % Show Material materials with Chrom of 0.1 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar | |
Eisen | 0.15 - 0.35 % Show Material materials with Eisen of 0.15 - 0.35 % | H111 | EN 573-3 | Rod, Tube |
0.35 % Show Material materials with Eisen of 0.35 % | H111 | EN 573-3 | Rod, Tube | |
0.35 % Show Material materials with Eisen of 0.35 % | H111 | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
0.6 - 0.9 % Show Material materials with Magnesium of 0.6 - 0.9 % | H111 | EN 573-3 | Rod, Tube | |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
0.15 % Show Material materials with Mangan of 0.15 % | H111 | EN 573-3 | Rod, Tube | |
Silizium | 0.2 - 0.6 % Show Material materials with Silizium of 0.2 - 0.6 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
0.3 - 0.6 % Show Material materials with Silizium of 0.3 - 0.6 % | H111 | EN 573-3 | Rod, Tube | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H111 | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Bar |
0.15 % Show Material materials with Zink of 0.15 % | H111 | EN 573-3 | Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): acceptable to poor / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good to acceptable, weathering: good | |
Workability | Excellent workability. |