Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Bending Fatigue Strength | 55.0 MPa Show Material materials with Bending Fatigue Strength of 55.0 MPa | O | AA Standards | ||
Dehnung | 16.0 % Show Material materials with Dehnung of 16.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | A50 |
16.0 % Show Material materials with Dehnung of 16.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A100 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | AA Standards, ASTM B221, ASTM B241, ASTM B345 | A50 | ||
18.0 % Show Material materials with Dehnung of 18.0 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Härte, Brinell | 25.0 [-] Show Material materials with Härte, Brinell of 25.0 [-] | O | AA Standards, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 6000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 6000 Series Aluminium | |||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 6000 Series Aluminium | |||
Zugfestigkeit | 90.0 MPa Show Material materials with Zugfestigkeit of 90.0 MPa | O | AA Standards | ||
130.0 MPa Show Material materials with Zugfestigkeit of 130.0 MPa | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
Schmelzpunkt | 600.0 °C Show Material materials with Schmelzpunkt of 600.0 °C | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
615.0 - 655.0 °C Show Material materials with Schmelzpunkt of 615.0 - 655.0 °C | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||||
Spezifische Wärmekapazität | 887.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 887.0 - 963.0 J/(kg·K) | Typical for Wrought 6000 Series Aluminium | ||||
Wärmeleitfähigkeit | 193.0 - 218.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 193.0 - 218.0 W/(m·K) | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |||
200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200.0 W/(m·K) | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 29000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 29000000.0 - 34000000.0 S/m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
spezifischer Widerstand | 2.94e-08 - 3.45e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.45e-08 Ω·m | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | |
3.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.5e-08 Ω·m | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | Total |
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Eisen | 0.35 % Show Material materials with Eisen of 0.35 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483 | ||
0.35 % Show Material materials with Eisen of 0.35 % | O | BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | ||
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Magnesium | 0.45 - 0.9 % Show Material materials with Magnesium of 0.45 - 0.9 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Silizium | 0.2 - 0.6 % Show Material materials with Silizium of 0.2 - 0.6 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | AA Standards, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B483, BS EN 573-3, BS EN 755-2, ASTM B210, ASTM B221, ASTM B241, ASTM B345, ASTM B361, ASTM B429, ASTM B483, ASTM B491, SAE J454 | Rod, Bar, Tube |
Technological properties
Property | ||
---|---|---|
Application areas | - 6063 Architectural, applications, Extrusions, Window frames, Doors, Shop fittings, Irrigation tubing, In balustrading the rails and posts are normally in the T6 temper and formed elbows and bends are T4. T4 temper 6063 aluminium is also finding applications in hydroformed tube for chassis. - 6063A 6063A is used in the same applications as 6063. It is also used in: Road transport Rail transport Extreme sports equipment | |
Brazing | general: possible with commercial processes and methods | |
Corrosion properties | Stress corrosion cracking: no damage during operation and laboratory tests, general: very good, without protection in industrial or seawater atmosphere | |
General machinability | General: poor (T1, T4), sufficient (T5, T452, T6, T83, T831, T832) | |
Soldering general | Good | |
Welding | 6063 is suitable for all conventional welding methods. Welding wire generally should be alloy 5183 or alloy 4043. When maximum electrical conductivity is required use alloy 4043. For strength and conductivity use alloy 5346 and increase the size of the weld to compensate for the lower conductivity. Gas: Excellent; Arc:Excellent; Resistance:Excellent. | |
Workability | general (condition): acceptable (T1, T4, T5, T452), poor(T6, T83, T831, T832) |