Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.77 g/cm³ Show Material materials with Dichte of 2.77 g/cm³ | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 2.77 g/cm³ Show Material materials with Dichte of 2.77 g/cm³ | T651 | EN 573-3 | Flat, Sheet |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 90° | 3.5 °/t Show Material materials with Biegewinkel 90° of 3.5 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
4.0 °/t Show Material materials with Biegewinkel 90° of 4.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
5.5 °/t Show Material materials with Biegewinkel 90° of 5.5 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
8.0 °/t Show Material materials with Biegewinkel 90° of 8.0 °/t | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
Dehnung | 5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | |
6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A100 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | A50 | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T651 | EN 573-3 | |||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T651 | EN 573-3 | Flat | A50 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Sheet | ||
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T651 | EN 573-3 | Sheet, Flat | A50 | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | T651 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | T651 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | T651 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 68.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 68.0 - 70.0 GPa | T651 | EN 573-3 | Flat, Sheet | ||
Härte, Brinell | 98.0 [-] Show Material materials with Härte, Brinell of 98.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
101.0 [-] Show Material materials with Härte, Brinell of 101.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
104.0 [-] Show Material materials with Härte, Brinell of 104.0 [-] | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 98.0 - 104.0 [-] Show Material materials with Härte, Brinell of 98.0 - 104.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 98.0 - 101.0 [-] Show Material materials with Härte, Brinell of 98.0 - 101.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 98.0 [-] Show Material materials with Härte, Brinell of 98.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 101.0 - 104.0 [-] Show Material materials with Härte, Brinell of 101.0 - 104.0 [-] | T651 | EN 573-3 | Flat | ||
20.0 °C | 101.0 [-] Show Material materials with Härte, Brinell of 101.0 [-] | T651 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 104.0 [-] Show Material materials with Härte, Brinell of 104.0 [-] | T651 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 26.4 GPa Show Material materials with Schubmodule of 26.4 GPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Schubmodule of 25.0 - 27.0 GPa | T651 | EN 573-3 | Flat, Sheet | ||
Zugfestigkeit | 330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | ||
340.0 MPa Show Material materials with Zugfestigkeit of 340.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
350.0 MPa Show Material materials with Zugfestigkeit of 350.0 MPa | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |||
20.0 °C | 330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 330.0 MPa Show Material materials with Zugfestigkeit of 330.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 340.0 MPa Show Material materials with Zugfestigkeit of 340.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 340.0 MPa Show Material materials with Zugfestigkeit of 340.0 MPa | T651 | EN 573-3 | Sheet | ||
20.0 °C | 350.0 MPa Show Material materials with Zugfestigkeit of 350.0 MPa | T651 | EN 573-3 | Flat | Transverse | |
20.0 °C | 350.0 MPa Show Material materials with Zugfestigkeit of 350.0 MPa | T651 | EN 573-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat |
-50.0 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
100 °C | 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
100.0 °C | 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
200 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
200.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Flat | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
300.0 °C | 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K | T651 | EN 573-3 | Flat, Sheet | |
Schmelzpunkt | 600.0 - 650.0 °C Show Material materials with Schmelzpunkt of 600.0 - 650.0 °C | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
Spezifische Wärmekapazität | 875.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 875.0 J/(kg·K) | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
20.0 °C | 875.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 875.0 J/(kg·K) | T651 | EN 573-3 | Flat, Sheet | |
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 160.0 W/(m·K) | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 23000000.0 S/m | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
spezifischer Widerstand | 4.35e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5.26e-08 Ω·m | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 - 0.35 % Show Material materials with Chrom of 0.1 - 0.35 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | T651 | EN 573-3 | Flat, Sheet |
0.40 % Show Material materials with Eisen of 0.40 % | T651 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube | |
Kupfer | 0.2 % Show Material materials with Kupfer of 0.2 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Magnesium | 1.0 - 1.4 % Show Material materials with Magnesium of 1.0 - 1.4 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Mangan | 0.05 - 0.5 % Show Material materials with Mangan of 0.05 - 0.5 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Silizium | 0.35 % Show Material materials with Silizium of 0.35 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Zink | 4.0 - 5.0 % Show Material materials with Zink of 4.0 - 5.0 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Zirkonium | 0.08 - 0.2 % Show Material materials with Zirkonium of 0.08 - 0.2 % | T651 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: good | |
Brazing | hard brazing (with flux/ without flux): not suitable / not suitable, friction soldering: acceptable, soft brazing with flux: not suitable | |
Corrosion properties | Seawater: sufficient, weathering: acceptable | |
Workability | Bending / Spinning (cold): good (O) / acceptable (O), Impact extrusion (cold): acceptable (O), Deep drawing / upsetting (Condition) good (O) / good (O) |