Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.84 g/cm³ Show Material materials with Dichte of 2.84 g/cm³ | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 3.0 % Show Material materials with Dehnung of 3.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A100 | |
4.0 % Show Material materials with Dehnung of 4.0 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3, EN 755 | Rod, Tube | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | T6510 | EN 573-3, EN 754 | Rod, Tube | A100 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | T6510 | EN 573-3 | Rod | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T6510 | EN 573-3 | Tube, Profile, Rod | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3 | Tube | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T6510 | EN 573-3 | Tube, Profile, Rod | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T6510 | EN 573-3 | Tube | ||
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | T6510 | EN 573-3 | Tube | ||
Elastizitätsmodul | 69.0 - 72.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 72.0 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Härte, Brinell | 20.0 °C | 170.0 [-] Show Material materials with Härte, Brinell of 170.0 [-] | T6510 | EN 573-3 | Tube, Profile, Rod | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 7000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 7000 Series Aluminium | ||||
Schubmodule | 26.4 - 27.1 GPa Show Material materials with Schubmodule of 26.4 - 27.1 GPa | Typical for Wrought 7000 Series Aluminium | ||||
Zugfestigkeit | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | ||
520.0 MPa Show Material materials with Zugfestigkeit of 520.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
560.0 MPa Show Material materials with Zugfestigkeit of 560.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
590.0 MPa Show Material materials with Zugfestigkeit of 590.0 MPa | T6510 | EN 573-3, EN 754 | Rod, Tube | |||
610.0 MPa Show Material materials with Zugfestigkeit of 610.0 MPa | T6510 | EN 573-3, EN 755 | Rod, Tube | |||
20.0 °C | 450.0 MPa Show Material materials with Zugfestigkeit of 450.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 520.0 MPa Show Material materials with Zugfestigkeit of 520.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 560.0 MPa Show Material materials with Zugfestigkeit of 560.0 MPa | T6510 | EN 573-3 | Rod | ||
20.0 °C | 590.0 MPa Show Material materials with Zugfestigkeit of 590.0 MPa | T6510 | EN 573-3 | Tube | ||
20.0 °C | 610.0 MPa Show Material materials with Zugfestigkeit of 610.0 MPa | T6510 | EN 573-3 | Tube, Profile, Rod |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.1e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 - 2.4e-05 1/K | Typical for Wrought 7000 Series Aluminium |
Schmelzpunkt | 465.0 - 655.0 °C Show Material materials with Schmelzpunkt of 465.0 - 655.0 °C | Typical for Wrought 7000 Series Aluminium |
Spezifische Wärmekapazität | 795.0 - 1050.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 795.0 - 1050.0 J/(kg·K) | Typical for Wrought 7000 Series Aluminium |
Wärmeleitfähigkeit | 121.0 - 170.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 121.0 - 170.0 W/(m·K) | Typical for Wrought 7000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 34000000.0 S/m | Typical for Wrought 7000 Series Aluminium |
spezifischer Widerstand | 2.9e-08 - 5.6e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 - 5.6e-08 Ω·m | Typical for Wrought 7000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.05 - 0.25 % Show Material materials with Chrom of 0.05 - 0.25 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | T6510 | EN 573-3 | Rod, Tube, Profile |
0.50 % Show Material materials with Eisen of 0.50 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube | |
Kupfer | 1.2 - 1.9 % Show Material materials with Kupfer of 1.2 - 1.9 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Magnesium | 2.1 - 3.1 % Show Material materials with Magnesium of 2.1 - 3.1 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Zink | 7.2 - 8.4 % Show Material materials with Zink of 7.2 - 8.4 % | T6510 | EN 573-3, EN 754, EN 755 | Rod, Tube, Profile |
Technological properties
Property | ||
---|---|---|
Brazing | Excellent |