Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire |
Abmessung
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Dicke | 0.2 mm Show Material materials with Dicke of 0.2 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | 0.2 mm | Coil, Sheet, Strip |
200 mm Show Material materials with Dicke of 200 mm | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | 200 mm | Coil, Sheet, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 25.0 MPa Show Material materials with Bending Fatigue Strength of 25.0 MPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Biegewinkel 180° | 0 °/t Show Material materials with Biegewinkel 180° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | ||
0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Biegewinkel 90° | 0 °/t Show Material materials with Biegewinkel 90° of 0 °/t | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | ||
0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | |
2.0 % Show Material materials with Dehnung of 2.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 - 20.0 % Show Material materials with Dehnung of 4.0 - 20.0 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 546, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3, EN 1396, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
23.0 % Show Material materials with Dehnung of 23.0 % | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
26.0 % Show Material materials with Dehnung of 26.0 % | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
29.0 % Show Material materials with Dehnung of 29.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
32.0 % Show Material materials with Dehnung of 32.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Foil | A50 | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | O | EN 573-3 | Foil | A100 | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Flat, Sheet, Strip | A50 Transverse | |
20.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 | |
20.0 °C | 22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3 | Flat, Sheet, Strip | A50 Transverse | |
20.0 °C | 22.0 % Show Material materials with Dehnung of 22.0 % | O | EN 573-3 | Rod, Tube, Sheet, Strip, Flat | A50 | |
20.0 °C | 23.0 % Show Material materials with Dehnung of 23.0 % | O | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 25.0 % Show Material materials with Dehnung of 25.0 % | O | EN 573-3 | Rod, Tube | ||
20.0 °C | 26.0 % Show Material materials with Dehnung of 26.0 % | O | EN 573-3 | Flat, Sheet, Strip | A50 Transverse | |
20.0 °C | 26.0 % Show Material materials with Dehnung of 26.0 % | O | EN 573-3 | Sheet, Strip, Flat | A50 | |
20.0 °C | 29.0 % Show Material materials with Dehnung of 29.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 29.0 % Show Material materials with Dehnung of 29.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 32.0 % Show Material materials with Dehnung of 32.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 32.0 % Show Material materials with Dehnung of 32.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3 | Wire | A100 | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3 | Flat | A50 | |
20.0 °C | 35.0 % Show Material materials with Dehnung of 35.0 % | O | EN 573-3 | Sheet, Strip | ||
Elastizitätsmodul | -270 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
-270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
-195.0 °C | 78.4 GPa Show Material materials with Elastizitätsmodul of 78.4 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
-85.0 °C | 73.5 GPa Show Material materials with Elastizitätsmodul of 73.5 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
-30.0 °C | 71.4 GPa Show Material materials with Elastizitätsmodul of 71.4 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 60.0 - 69.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 69.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2, EN 573-3 | Coil, Sheet, Strip, Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
100.0 °C | 68.0 - 68.6 GPa Show Material materials with Elastizitätsmodul of 68.0 - 68.6 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
100.0 °C | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
150.0 °C | 66.0 - 66.5 GPa Show Material materials with Elastizitätsmodul of 66.0 - 66.5 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
150.0 °C | 66.5 GPa Show Material materials with Elastizitätsmodul of 66.5 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
250.0 °C | 56.0 - 57.0 GPa Show Material materials with Elastizitätsmodul of 56.0 - 57.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
250.0 °C | 56.0 GPa Show Material materials with Elastizitätsmodul of 56.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
300 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
Härte, Brinell | 20.0 [-] Show Material materials with Härte, Brinell of 20.0 [-] | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 20.0 [-] Show Material materials with Härte, Brinell of 20.0 [-] | O | EN 573-3 | Flat, Rod, Tube | ||
Härte, HBW | 20 [-] Show Material materials with Härte, HBW of 20 [-] | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | |
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 25.0 - 26.5 GPa Show Material materials with Schubmodule of 25.0 - 26.5 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 25.0 - 25.9 GPa Show Material materials with Schubmodule of 25.0 - 25.9 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 25.9 - 26.5 GPa Show Material materials with Schubmodule of 25.9 - 26.5 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
Streckgrenze | -270 °C | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | O | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 |
-270.0 °C | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | O | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
20.0 MPa Show Material materials with Streckgrenze of 20.0 MPa | O | EN 573-3, EN 1396, EN 485, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
20 MPa Show Material materials with Streckgrenze of 20 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |||
55.0 MPa Show Material materials with Streckgrenze of 55.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP02 | ||
20.0 °C | 20.0 MPa Show Material materials with Streckgrenze of 20.0 MPa | O | EN 573-3 | Flat, Sheet, Strip | RP02 Transverse | |
20.0 °C | 20.0 - 60.0 MPa Show Material materials with Streckgrenze of 20.0 - 60.0 MPa | O | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 20.0 MPa Show Material materials with Streckgrenze of 20.0 MPa | O | EN 573-3 | Rod, Tube, Sheet, Strip, Flat | RP02 | |
20.0 °C | 20.0 - 55.0 MPa Show Material materials with Streckgrenze of 20.0 - 55.0 MPa | O | EN 573-3 | Sheet, Strip, Plate, Foil, Bar, Rod, Tube | RP02 | |
20.0 °C | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | O | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
20 °C | 30.0 MPa Show Material materials with Streckgrenze of 30.0 MPa | O | EN 573-3 | Rod, Sheet, Strip, Tube, Plate, Foil, Bar | RP1 | |
20.0 °C | 55.0 MPa Show Material materials with Streckgrenze of 55.0 MPa | O | EN 573-3 | Foil | RP02 | |
50.0 °C | 29.0 MPa Show Material materials with Streckgrenze of 29.0 MPa | O | EN 573-3 | RP1 | ||
100 °C | 13.0 MPa Show Material materials with Streckgrenze of 13.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | RP1 | |
100.0 °C | 27.0 MPa Show Material materials with Streckgrenze of 27.0 MPa | O | EN 573-3 | RP1 | ||
Zugfestigkeit | 60.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 80.0 MPa | O | EN 573-3, EN 1715-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
60.0 MPa Show Material materials with Zugfestigkeit of 60.0 MPa | O | EN 573-3, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
65.0 MPa Show Material materials with Zugfestigkeit of 65.0 MPa | O | EN 573-3 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | O | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 35.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 35.0 - 80.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 35.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 35.0 - 85.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 35.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 35.0 - 90.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 35.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 35.0 - 95.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 40.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 40.0 - 85.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 40.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 40.0 - 80.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 40.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 40.0 - 90.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 40.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 40.0 - 95.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 45.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 90.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 45.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 95.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 45.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 80.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 45.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 45.0 - 85.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 50.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 95.0 MPa | O | EN 573-3, EN 546, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Coil, Sheet, Strip | ||
20.0 °C | 50.0 - 80.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 80.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 50.0 - 85.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 85.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 50.0 - 90.0 MPa Show Material materials with Zugfestigkeit of 50.0 - 90.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 60.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 95.0 MPa | O | EN 573-3, EN 754, EN 755 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 65.0 - 95.0 MPa | O | EN 573-3 | Flat, Sheet, Strip | Transverse | |
20.0 °C | 65.0 MPa Show Material materials with Zugfestigkeit of 65.0 MPa | O | EN 573-3 | Rod, Sheet, Strip, Tube | ||
20.0 °C | 65.0 - 95.0 MPa Show Material materials with Zugfestigkeit of 65.0 - 95.0 MPa | O | EN 573-3, EN 1396, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat | ||
20.0 °C | 95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | O | EN 573-3 | Wire |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | |
-50.0 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
100.0 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | 20-100°C | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
200.0 °C | 2.44e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.44e-05 1/K | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
300.0 °C | 2.54e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.54e-05 1/K | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
Schmelzpunkt | 646.0 - 657.0 °C Show Material materials with Schmelzpunkt of 646.0 - 657.0 °C | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 899.0 - 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 - 900.0 J/(kg·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 J/(kg·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | ||
20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire | ||
20.0 °C | 210.0 - 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 229.0 W/(m·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 220.0 - 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 220.0 - 229.0 W/(m·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | ||
20.0 °C | 229.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 229.0 W/(m·K) | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 34000000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 36000000.0 S/m | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 34800000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34800000.0 - 36000000.0 S/m | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | |
spezifischer Widerstand | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.94e-08 Ω·m | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
4.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.9e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | ||
20.0 °C | 2.8e-08 - 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.8e-08 - 2.9e-08 Ω·m | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire | |
20.0 °C | 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.9e-08 Ω·m | O | EN 573-3 | Sheet, Strip, Foil, Rod, Flat, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar |
Andere | 0.03 % Show Material materials with Andere of 0.03 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip |
Bor | 0.05 Show Material materials with Bor of 0.05 | O | EN 573-3 | Flat |
Chrom | 0.01 Show Material materials with Chrom of 0.01 | O | EN 573-3 | Flat |
Eisen | 0.4 % Show Material materials with Eisen of 0.4 % | O | EN 573-3 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire |
0.40 % Show Material materials with Eisen of 0.40 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
0.4 % Show Material materials with Eisen of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Gallium | 0.03 Show Material materials with Gallium of 0.03 | O | EN 573-3 | Flat |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar |
0.05 % Show Material materials with Kupfer of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Magnesium | 0.03 % Show Material materials with Magnesium of 0.03 % | O | EN 573-3 | Flat |
0.05 % Show Material materials with Magnesium of 0.05 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar | |
0.05 % Show Material materials with Magnesium of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | O | EN 573-3 | Flat |
0.05 % Show Material materials with Mangan of 0.05 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar | |
0.05 % Show Material materials with Mangan of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Nickel | 0.03 Show Material materials with Nickel of 0.03 | O | EN 573-3 | Flat |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | O | EN 573-3 | Flat |
0.25 % Show Material materials with Silizium of 0.25 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar | |
0.25 % Show Material materials with Silizium of 0.25 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | O | EN 573-3 | Flat |
0.05 % Show Material materials with Titan of 0.05 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar | |
0.05 % Show Material materials with Titan of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip | |
Vanadium | 0.03 Show Material materials with Vanadium of 0.03 | O | EN 573-3 | Flat |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | O | EN 573-3 | Flat |
0.07 % Show Material materials with Zink of 0.07 % | O | EN 573-3, EN 1301, EN 1396, EN 1715-3, EN 485, EN 546, EN 683, EN 754, EN 755 | Flat, Sheet, Strip, Foil, Rod, Tube, Wire, Plate, Bar | |
0.07 % Show Material materials with Zink of 0.07 % | O | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 683-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | Excellent | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Lithography; Cable Wrapping: Electric cable wrapping; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors, Photovoltaic panels; Wind energy: Nacelle coverings, rotor hub, stairs; Cosmetics: Cosmetics pieces; Automotive Trim: Interior Trim, Marque Badges; Components: Heat shields, General Transportation | |
Brazing | Excellent | |
Corrosion properties | Excellent | |
Welding | Excellent | |
Workability | Excellent |