Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Schubmodule | 25.9 GPa Show Material materials with Schubmodule of 25.9 GPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Zugfestigkeit | 105.0 - 145.0 MPa Show Material materials with Zugfestigkeit of 105.0 - 145.0 MPa | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
20 °C | 2.17e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.17e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
200 °C | 2.4399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4399999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
300 °C | 2.5399999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5399999999999997e-05 1/K | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Schmelzpunkt | 646.0 - 657.0 °C Show Material materials with Schmelzpunkt of 646.0 - 657.0 °C | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Spezifische Wärmekapazität | 900.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 J/(kg·K) | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Wärmeleitfähigkeit | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 34000000.0 - 36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 36000000.0 S/m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
spezifischer Widerstand | 2.78e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 - 2.94e-08 Ω·m | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eisen | 0.40 % Show Material materials with Eisen of 0.40 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Silizium | 0.25 % Show Material materials with Silizium of 0.25 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Zink | 0.07 % Show Material materials with Zink of 0.07 % | H244 | EN 573-3, EN 1386 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: acceptable, weathering: good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |