Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
7.0 % Show Material materials with Dehnung of 7.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | A50 | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Wire | A100 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 7.0 % Show Material materials with Dehnung of 7.0 % | H14 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Flat, Wire | |
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |||
20.0 °C | 60.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 60.0 - 70.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H14 | EN 573-3 | Flat, Wire | ||
Härte, Brinell | 32.0 [-] Show Material materials with Härte, Brinell of 32.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 32.0 [-] Show Material materials with Härte, Brinell of 32.0 [-] | H14 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 25.0 - 26.5 GPa Show Material materials with Schubmodule of 25.0 - 26.5 GPa | H14 | EN 573-3 | Flat, Wire | |
Zugfestigkeit | 95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Wire, Tube, Bar | ||
20.0 °C | 95.0 MPa Show Material materials with Zugfestigkeit of 95.0 MPa | H14 | EN 573-3 | Wire | ||
20.0 °C | 100.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 140.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 100.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 100.0 - 140.0 MPa | H14 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Wire, Tube, Bar |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Schmelzpunkt | 659.0 °C Show Material materials with Schmelzpunkt of 659.0 °C | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Spezifische Wärmekapazität | 20.0 °C | 921.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 921.0 J/(kg·K) | H14 | EN 573-3 | Flat, Wire |
Wärmeleitfähigkeit | 225 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 225 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |
20.0 °C | 215.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 215.0 W/(m·K) | H14 | EN 573-3 | Flat, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 34500000.0 - 35000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34500000.0 - 35000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |
20.0 °C | 35800000.0 - 36800000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 35800000.0 - 36800000.0 S/m | H14 | EN 573-3 | Flat, Wire | |
spezifischer Widerstand | 2.86e-08 - 2.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.86e-08 - 2.9e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.7 % Show Material materials with Aluminium of 99.7 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Eisen | 0.25 % Show Material materials with Eisen of 0.25 % | H14 | EN 573-3 | Flat, Wire |
0.25 % Show Material materials with Eisen of 0.25 % | H14 | EN 573-3, EN 1301, EN 485 | Strip, Sheet, Plate, Wire, Tube, Bar | |
Kupfer | 0.03 % Show Material materials with Kupfer of 0.03 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Magnesium | 0.03 % Show Material materials with Magnesium of 0.03 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Mangan | 0.03 % Show Material materials with Mangan of 0.03 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Silizium | 0.2 % Show Material materials with Silizium of 0.2 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Titan | 0.03 % Show Material materials with Titan of 0.03 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Zink | 0.07 % Show Material materials with Zink of 0.07 % | H14 | EN 573-3, EN 1301, EN 485 | Flat, Wire, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: very good, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): very good, Deep drawing / upsetting (Condition) very good (H14) / very good (H12) |