Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | O | EN 573-3, EN 683 | Strip, Sheet |
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-3, EN 683 | Strip, Sheet | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | ||||
Schubmodule | 26.0 GPa Show Material materials with Schubmodule of 26.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | ||
Zugfestigkeit | 20.0 °C | 60.0 - 105.0 MPa Show Material materials with Zugfestigkeit of 60.0 - 105.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet, Foil |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 683 | Strip, Sheet | |
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | O | EN 573-3, EN 683 | Strip, Sheet | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | 20-100°C | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | O | EN 573-3, EN 683 | Strip, Sheet | ||
Spezifische Wärmekapazität | 900.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Wärmeleitfähigkeit | 218.0 - 222.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 218.0 - 222.0 W/(m·K) | O | EN 573-3, EN 683 | Strip, Sheet | ||
218 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 218 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | |||
222.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 222.0 W/(m·K) | O | EN 573-3, EN 683 | Strip, Sheet |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 33000000.0 - 34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 33000000.0 - 34000000.0 S/m | O | EN 573-3, EN 683 | Strip, Sheet |
34000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 S/m | O | EN 573-3, EN 683 | Strip, Sheet | |
spezifischer Widerstand | 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 Ω·m | O | EN 573-3, EN 683 | Strip, Sheet |
2.94e-08 - 3.03e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.94e-08 - 3.03e-08 Ω·m | O | EN 573-3, EN 683 | Strip, Sheet | |
3.0000000000000004e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.0000000000000004e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil |
Chemical properties
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Aluminium | 99.0 % Show Material materials with Aluminium of 99.0 % | O | EN 573-3, EN 683 | Foil, Strip, Sheet | |
Andere | 0.15 % Show Material materials with Andere of 0.15 % | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | |
Eisen | 0.95 % Show Material materials with Eisen of 0.95 % | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | Si + Fe |
Kupfer | 0.05 - 0.2 % Show Material materials with Kupfer of 0.05 - 0.2 % | O | EN 573-3, EN 683, EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Foil, Strip, Sheet, Coil, Sheet, Foil | |
Mangan | 0.05 % Show Material materials with Mangan of 0.05 % | O | EN 573-3, EN 683 | Foil, Strip, Sheet | |
0.05 % Show Material materials with Mangan of 0.05 % | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | ||
Silizium | 0.95 % Show Material materials with Silizium of 0.95 % | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil | Si + Fe |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | EN 573-3, EN 683 | Foil, Strip, Sheet | |
0.1 % Show Material materials with Zink of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 683-2, ASTM B 209 | Coil, Sheet, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | Very Good | |
Application areas | Roofing: Foil for bituminous coating; Interiors and ceilings: Decoration; Lighting: Anodizing Quality, Lacquering quality; Electronic devices: Housing of devices; Heat exchangers: Fins, General applications; Tubes: Industrial tubes, Flexible tube, Pipes; Insulation; Solar: Solar collectors; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Components: Automotive fins, Heat exchangers | |
Brazing | Excellent | |
Corrosion properties | Very Good | |
Welding | Excellent | |
Workability | Excellent |