Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
2.705 g/cm³ Show Material materials with Dichte of 2.705 g/cm³ | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Abmessung
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | |
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | |
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H12 | EN 573-3, EN 485 | Plate, Rod | ||
3 °/t Show Material materials with Biegewinkel 90° of 3 °/t | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 |
4.0 % Show Material materials with Dehnung of 4.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
5.0 % Show Material materials with Dehnung of 5.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
7.0 % Show Material materials with Dehnung of 7.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | A50 | |
9.0 % Show Material materials with Dehnung of 9.0 % | H12 | EN 573-3, EN 485 | Plate, Rod | ||
20.0 % Show Material materials with Dehnung of 20.0 % | H12 | EN 573-3, EN 1715-2 | Plate, Rod | A50 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
Härte, Brinell | 28.0 [-] Show Material materials with Härte, Brinell of 28.0 [-] | H12 | EN 573-3, EN 485 | Plate, Rod | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 1000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 1000 Series Aluminium | |||
Schubmodule | 26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zugfestigkeit | 85.0 - 125.0 MPa Show Material materials with Zugfestigkeit of 85.0 - 125.0 MPa | H12 | EN 573-3, EN 485 | Plate, Rod | |
95.0 - 110.0 MPa Show Material materials with Zugfestigkeit of 95.0 - 110.0 MPa | H12 | EN 573-3, EN 1715-2 | Plate, Rod |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | 20-100°C | |
Schmelzpunkt | 645.0 - 657.0 °C Show Material materials with Schmelzpunkt of 645.0 - 657.0 °C | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | ||
645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |||
Spezifische Wärmekapazität | 900.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 900.0 - 963.0 J/(kg·K) | Typical for Wrought 1000 Series Aluminium | ||||
Wärmeleitfähigkeit | 138 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 138 W/(m·K) | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | ||
225.0 - 235.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 225.0 - 235.0 W/(m·K) | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |||
234 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 234 W/(m·K) | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 35400000.0 - 36500000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 35400000.0 - 36500000.0 S/m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
36000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 36000000.0 S/m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
spezifischer Widerstand | 2.74e-08 - 2.82e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.74e-08 - 2.82e-08 Ω·m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
2.78e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.78e-08 Ω·m | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod | |
4.9e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.9e-08 Ω·m | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 99.5 % Show Material materials with Aluminium of 99.5 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Andere | 0.1 % Show Material materials with Andere of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Bor | 0.05 % Show Material materials with Bor of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Chrom | 0.01 % Show Material materials with Chrom of 0.01 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.01 % Show Material materials with Chrom of 0.01 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Eisen | 0.40 % Show Material materials with Eisen of 0.40 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.4 % Show Material materials with Eisen of 0.4 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Gallium | 0.03 % Show Material materials with Gallium of 0.03 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.05 % Show Material materials with Kupfer of 0.05 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Mangan | 0.01 % Show Material materials with Mangan of 0.01 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.01 % Show Material materials with Mangan of 0.01 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Silizium | 0.1 % Show Material materials with Silizium of 0.1 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.1 % Show Material materials with Silizium of 0.1 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet | |
Zink | 0.05 % Show Material materials with Zink of 0.05 % | H12 | EN 573-3, EN 1715-2, EN 485 | Plate, Rod |
0.05 % Show Material materials with Zink of 0.05 % | H12 | EN 573-1, EN 573-2, EN 573-3, EN 485-2 | Coil, Sheet |
Technological properties
Property | ||
---|---|---|
Anodizing | Good (For surface protection only) | |
Application areas | Conductors; rods for the manufacture of aluminium conductor wires. | |
Brazing | Excellent | |
Corrosion properties | Very Good | |
Welding | Very Good | |
Workability | Very Good |