Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
2.83 g/cm³ Show Material materials with Dichte of 2.83 g/cm³ | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | H13 | EN 573-3 | Wire |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
72.5 GPa Show Material materials with Elastizitätsmodul of 72.5 GPa | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | |||
Schubmodule | 27.3 GPa Show Material materials with Schubmodule of 27.3 GPa | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
Zugfestigkeit | 155.0 - 225.0 MPa Show Material materials with Zugfestigkeit of 155.0 - 225.0 MPa | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire |
-50.0 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire | |
20 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
100.0 °C | 2.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.29e-05 1/K | H13 | EN 573-3 | Wire | |
100.0 °C | 2.29e-05 - 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.29e-05 - 2.31e-05 1/K | H13 | EN 573-3 | Wire | |
100.0 °C | 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | H13 | EN 573-3 | Wire | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
200 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire | |
200.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar, Wire | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
300.0 °C | 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K | H13 | EN 573-3 | Wire | |
Schmelzpunkt | 540.0 - 645.0 °C Show Material materials with Schmelzpunkt of 540.0 - 645.0 °C | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | H13 | EN 573-3 | Wire | |
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 151.0 - 172.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 151.0 - 172.0 W/(m·K) | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 32000000.0 S/m | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 23000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 26000000.0 S/m | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar | |
spezifischer Widerstand | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-08 - 4.17e-08 Ω·m | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 4.35e-08 Ω·m | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismut | 0.2 - 0.6 % Show Material materials with Bismut of 0.2 - 0.6 % | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Blei | 0.2 - 0.6 % Show Material materials with Blei of 0.2 - 0.6 % | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H13 | EN 573-3 | Wire |
0.70 % Show Material materials with Eisen of 0.70 % | H13 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 5.0 - 6.0 % Show Material materials with Kupfer of 5.0 - 6.0 % | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Zink | 0.3 % Show Material materials with Zink of 0.3 % | H13 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: poor | |
Brazing | hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient | |
Corrosion properties | Seawater: poor, weathering: sufficient | |
Workability | Deep drawing / upsetting (Condition) - / acceptable |