Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
2.83 g/cm³ Show Material materials with Dichte of 2.83 g/cm³ | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 2.82 g/cm³ Show Material materials with Dichte of 2.82 g/cm³ | T8 | EN 573-3 | Rod, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | T8 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Tube, Bar | ||
6.0 % Show Material materials with Dehnung of 6.0 % | T8 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A50 | ||
8.0 % Show Material materials with Dehnung of 8.0 % | T8 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Bar | A100 | ||
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T8 | EN 573-3 | Rod, Tube | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | T8 | EN 573-3 | Wire | A100 | |
20.0 °C | 8.0 % Show Material materials with Dehnung of 8.0 % | T8 | EN 573-3 | Rod, Tube | ||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
72.5 GPa Show Material materials with Elastizitätsmodul of 72.5 GPa | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |||
Härte, Brinell | 20.0 °C | 115.0 [-] Show Material materials with Härte, Brinell of 115.0 [-] | T8 | EN 573-3 | Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 27.3 GPa Show Material materials with Schubmodule of 27.3 GPa | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
Zugfestigkeit | 370.0 MPa Show Material materials with Zugfestigkeit of 370.0 MPa | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T8 | EN 573-3 | Wire | ||
20.0 °C | 370.0 MPa Show Material materials with Zugfestigkeit of 370.0 MPa | T8 | EN 573-3 | Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire |
-50.0 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire | |
20 °C | 2.14e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.14e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire | |
20 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire | |
20 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
100.0 °C | 2.29e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.29e-05 1/K | T8 | EN 573-3 | Rod, Tube, Wire | |
100.0 °C | 2.29e-05 - 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.29e-05 - 2.31e-05 1/K | T8 | EN 573-3 | Rod, Tube, Wire | |
100.0 °C | 2.31e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.31e-05 1/K | T8 | EN 573-3 | Rod, Tube, Wire | |
100 °C | 2.3399999999999996e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3399999999999996e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
200 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire | |
200.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar, Rod, Wire | |
300 °C | 2.4999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4999999999999998e-05 1/K | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
300.0 °C | 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.5e-05 1/K | T8 | EN 573-3 | Rod, Tube, Wire | |
Schmelzpunkt | 540.0 - 645.0 °C Show Material materials with Schmelzpunkt of 540.0 - 645.0 °C | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
585.0 - 650.0 °C Show Material materials with Schmelzpunkt of 585.0 - 650.0 °C | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 864.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 864.0 J/(kg·K) | T8 | EN 573-3 | Rod, Tube, Wire | |
Wärmeleitfähigkeit | 170.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 170.0 - 220.0 W/(m·K) | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 151.0 - 172.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 151.0 - 172.0 W/(m·K) | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 24000000.0 - 32000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 - 32000000.0 S/m | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 23000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 26000000.0 S/m | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar | |
spezifischer Widerstand | 3.13e-08 - 4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.13e-08 - 4.17e-08 Ω·m | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
3.85e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 4.35e-08 Ω·m | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Bismut | 0.2 - 0.6 % Show Material materials with Bismut of 0.2 - 0.6 % | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Blei | 0.2 - 0.6 % Show Material materials with Blei of 0.2 - 0.6 % | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | T8 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Eisen of 0.7 % | T8 | EN 573-3 | Rod, Tube, Wire | |
0.70 % Show Material materials with Eisen of 0.70 % | T8 | EN 573-3, EN 1301, EN 754 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 4.5 - 6.0 % Show Material materials with Kupfer of 4.5 - 6.0 % | T8 | EN 573-3 | Rod, Tube |
5.0 - 6.0 % Show Material materials with Kupfer of 5.0 - 6.0 % | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar | |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Zink | 0.3 % Show Material materials with Zink of 0.3 % | T8 | EN 573-3, EN 1301, EN 754 | Rod, Tube, Wire, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not suitable, Protective: poor | |
Brazing | hard brazing (with flux/ without flux): not suitable /, friction soldering: sufficient | |
Corrosion properties | Seawater: poor, weathering: sufficient | |
Workability | Deep drawing / upsetting (Condition) - / acceptable |