Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.8 g/cm³ Show Material materials with Dichte of 2.8 g/cm³ | Typical for Cast 7xx.x Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | T1 | EN 1706 | Casting | ||
Elastizitätsmodul | 74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | Typical for Cast 7xx.x Series Aluminium | ||||
Härte, Brinell | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | T1 | EN 1706 | Casting | ||
65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | T1 | EN 1706 | Casting | |||
20.0 °C | 60.0 [-] Show Material materials with Härte, Brinell of 60.0 [-] | T1 | EN 1706 | |||
20.0 °C | 65.0 [-] Show Material materials with Härte, Brinell of 65.0 [-] | T1 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 7xx.x Series Aluminium | ||||
Zugfestigkeit | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | T1 | EN 1706 | Casting | ||
210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | T1 | EN 1706 | Casting | |||
20.0 °C | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | T1 | EN 1706 | |||
20.0 °C | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | T1 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T1 | EN 1706 | Casting | |
100.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T1 | EN 1706 | Casting | ||
100 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | T1 | EN 1706 | Casting | ||
Schmelzpunkt | 550.0 - 645.0 °C Show Material materials with Schmelzpunkt of 550.0 - 645.0 °C | Typical for Cast 7xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | Typical for Cast 7xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 140.0 W/(m·K) | T1 | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 19000000.0 - 21000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 21000000.0 S/m | T1 | EN 1706 | Casting |
spezifischer Widerstand | 4.76e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.76e-08 - 5.26e-08 Ω·m | T1 | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.3 % Show Material materials with Aluminium of 90.3 % | T1 | EN 1706 | |
Blei | 0.05 % Show Material materials with Blei of 0.05 % | T1 | EN 1706 | Casting |
Chrom | 0.15 - 0.6 % Show Material materials with Chrom of 0.15 - 0.6 % | T1 | EN 1706 | Casting |
Eisen | 0.8 % Show Material materials with Eisen of 0.8 % | T1 | EN 1706 | |
0.80 % Show Material materials with Eisen of 0.80 % | T1 | EN 1706 | Casting | |
Kupfer | 0.15 - 0.35 % Show Material materials with Kupfer of 0.15 - 0.35 % | T1 | EN 1706 | Casting |
Magnesium | 0.4 - 0.7 % Show Material materials with Magnesium of 0.4 - 0.7 % | T1 | EN 1706 | Casting |
Mangan | 0.4 % Show Material materials with Mangan of 0.4 % | T1 | EN 1706 | Casting |
Nickel | 0.05 % Show Material materials with Nickel of 0.05 % | T1 | EN 1706 | Casting |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | T1 | EN 1706 | Casting |
Titan | 0.1 - 0.25 % Show Material materials with Titan of 0.1 - 0.25 % | T1 | EN 1706 | Casting |
Zink | 4.5 - 6.0 % Show Material materials with Zink of 4.5 - 6.0 % | T1 | EN 1706 | Casting |
Zinn | 0.05 % Show Material materials with Zinn of 0.05 % | T1 | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: good | |
Corrosion properties | general: good | |
General machinability | after thermal treatment: excellent, as cast: excellent | |
Processing methods | permanent mould casting, separately cast test sample |