Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.77 g/cm³ Show Material materials with Dichte of 2.77 g/cm³ | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 4.0 % Show Material materials with Dehnung of 4.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | |
5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | T851 | EN 573-3 | Sheet | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | T851 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 70.0 - 73.0 GPa Show Material materials with Elastizitätsmodul of 70.0 - 73.0 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||||
Zugfestigkeit | 395.0 MPa Show Material materials with Zugfestigkeit of 395.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
405.0 MPa Show Material materials with Zugfestigkeit of 405.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T851 | EN 573-3, EN 485 | Strip, Sheet, Plate | |||
20.0 °C | 395.0 MPa Show Material materials with Zugfestigkeit of 395.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 395.0 MPa Show Material materials with Zugfestigkeit of 395.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 405.0 MPa Show Material materials with Zugfestigkeit of 405.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 405.0 MPa Show Material materials with Zugfestigkeit of 405.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 410.0 MPa Show Material materials with Zugfestigkeit of 410.0 MPa | T851 | EN 573-3 | Sheet | ||
20.0 °C | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T851 | EN 573-3 | Flat | Transverse | |
20.0 °C | 420.0 MPa Show Material materials with Zugfestigkeit of 420.0 MPa | T851 | EN 573-3 | Flat |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 1.6e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.6e-05 - 2.4e-05 1/K | Typical for Wrought 2000 Series Aluminium |
Schmelzpunkt | 500.0 - 650.0 °C Show Material materials with Schmelzpunkt of 500.0 - 650.0 °C | Typical for Wrought 2000 Series Aluminium |
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 251.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 251.0 W/(m·K) | Typical for Wrought 2000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 30000000.0 S/m | Typical for Wrought 2000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 6e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 6e-08 Ω·m | Typical for Wrought 2000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.9 - 1.4 % Show Material materials with Eisen of 0.9 - 1.4 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Kupfer | 1.8 - 2.7 % Show Material materials with Kupfer of 1.8 - 2.7 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Magnesium | 1.2 - 1.8 % Show Material materials with Magnesium of 1.2 - 1.8 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Mangan | 0.25 % Show Material materials with Mangan of 0.25 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Nickel | 0.8 - 1.4 % Show Material materials with Nickel of 0.8 - 1.4 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Silizium | 0.15 - 0.25 % Show Material materials with Silizium of 0.15 - 0.25 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | T851 | EN 573-3, EN 485 | Flat, Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Moderate Workability |