Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.74 g/cm³ Show Material materials with Dichte of 2.74 g/cm³ | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil |
2.74 g/cm³ Show Material materials with Dichte of 2.74 g/cm³ | O | EN 573-3, EN 546, EN 683, EN 1396 | Strip, Sheet |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 8000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 8000 Series Aluminium | ||||
Schubmodule | 25.0 GPa Show Material materials with Schubmodule of 25.0 GPa | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | ||
Streckgrenze | 45.0 MPa Show Material materials with Streckgrenze of 45.0 MPa | O | EN 573-3, EN 1396 | Strip, Sheet | RP02 | |
100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | O | EN 573-3, EN 683 | Strip, Sheet | RP02 | ||
100 MPa Show Material materials with Streckgrenze of 100 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | |||
20.0 °C | 45.0 MPa Show Material materials with Streckgrenze of 45.0 MPa | O | EN 573-3 | Sheet, Strip | RP02 Transverse | |
20.0 °C | 70.0 MPa Show Material materials with Streckgrenze of 70.0 MPa | O | EN 573-3 | Foil | RP02 | |
20.0 °C | 95.0 MPa Show Material materials with Streckgrenze of 95.0 MPa | O | EN 573-3 | Foil | RP02 | |
Zugfestigkeit | 70.0 MPa Show Material materials with Zugfestigkeit of 70.0 MPa | O | EN 573-3, EN 1396 | Strip, Sheet | ||
20.0 °C | 70.0 MPa Show Material materials with Zugfestigkeit of 70.0 MPa | O | EN 573-3 | Sheet, Strip | Transverse | |
20.0 °C | 80.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 135.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Foil | ||
20.0 °C | 80.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 80.0 - 140.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 85.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 85.0 - 140.0 MPa | O | EN 573-3, EN 546 | Strip, Sheet, Foil | ||
20.0 °C | 85.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 85.0 - 135.0 MPa | O | EN 573-3 | Foil | ||
20.0 °C | 90.0 - 140.0 MPa Show Material materials with Zugfestigkeit of 90.0 - 140.0 MPa | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 573-3, EN 546, EN 683 | Coil, Foil, Strip, Sheet, Foil | ||
20.0 °C | 90.0 - 135.0 MPa Show Material materials with Zugfestigkeit of 90.0 - 135.0 MPa | O | EN 573-3 | Foil |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | 20-100°C |
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | Typical for Wrought 8000 Series Aluminium | ||||
Spezifische Wärmekapazität | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | Typical for Wrought 8000 Series Aluminium | ||||
Wärmeleitfähigkeit | 190.0 - 210.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 190.0 - 210.0 W/(m·K) | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil |
Elektrisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 28000000.0 - 35000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 28000000.0 - 35000000.0 S/m | Typical for Wrought 8000 Series Aluminium | |||
spezifischer Widerstand | 3.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.1e-08 Ω·m | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 1.2 - 2.0 % Show Material materials with Eisen of 1.2 - 2.0 % | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil, Coil, Foil |
Kupfer | 0.3 % Show Material materials with Kupfer of 0.3 % | O | EN 573-3, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil |
0.3 % Show Material materials with Kupfer of 0.3 % | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | O | EN 573-3, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil |
0.1 % Show Material materials with Magnesium of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | |
Mangan | 0.3 - 1.0 % Show Material materials with Mangan of 0.3 - 1.0 % | O | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil, Coil, Foil |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | O | EN 573-3, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil |
0.4 % Show Material materials with Silizium of 0.4 % | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | O | EN 573-3, EN 546, EN 683, EN 1396 | Sheet, Strip, Foil |
0.1 % Show Material materials with Zink of 0.1 % | O | EN 573-1, EN 573-2, EN 573-3, EN 546-2, EN 683-2 | Coil, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | Limited | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels; Electronic devices: Housing of devices; Heat exchangers: Fins, Heat exchangers, General applications; Tubes: Industrial tubes, Flexible tubes, Pipes; Insulation; Semi-rigid and corrugated: Pet food, Smooth wall; Components: Automotive fins, Heat exchangers | |
Corrosion properties | Limited | |
Welding | Good | |
Workability | Very Good |