Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | |
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H24 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Foil, Sheet, Flat, Coil, Sheet, Strip, Foil |
Abmessung
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Dicke | 0.18 mm Show Material materials with Dicke of 0.18 mm | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | 0.18 mm | Coil, Sheet, Strip, Foil |
0.35 mm Show Material materials with Dicke of 0.35 mm | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | 0.35 mm | Coil, Sheet, Strip, Foil |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | |||
Härte, Brinell | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil | ||
20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | H24 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 8000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 8000 Series Aluminium | ||||
Schubmodule | 25.725 GPa Show Material materials with Schubmodule of 25.725 GPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | ||
Streckgrenze | 90.0 MPa Show Material materials with Streckgrenze of 90.0 MPa | H24 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil | RP02 | |
100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | H24 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil | RP02 | ||
110.0 - 140.0 MPa Show Material materials with Streckgrenze of 110.0 - 140.0 MPa | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | according to EN 485-2 | ||
20.0 °C | 90.0 MPa Show Material materials with Streckgrenze of 90.0 MPa | H24 | EN 573-3 | Foil | RP02 | |
20.0 °C | 100.0 - 140.0 MPa Show Material materials with Streckgrenze of 100.0 - 140.0 MPa | H24 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil | RP02 | |
20.0 °C | 100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | H24 | EN 573-3 | Foil, Flat | RP02 | |
20.0 °C | 100.0 MPa Show Material materials with Streckgrenze of 100.0 MPa | H24 | EN 573-3 | Flat | RP02 Transverse | |
Zugfestigkeit | 20.0 °C | 110.0 - 165.0 MPa Show Material materials with Zugfestigkeit of 110.0 - 165.0 MPa | H24 | EN 573-3, EN 546, EN 683 | Foil, Strip, Sheet, Plate | |
20.0 °C | 120.0 - 160.0 MPa Show Material materials with Zugfestigkeit of 120.0 - 160.0 MPa | H24 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2, EN 541 | Sheet, Coil, Sheet, Strip, Foil, Strip, Plate, Foil | according to EN 485-2 | |
20.0 °C | 120.0 - 170.0 MPa Show Material materials with Zugfestigkeit of 120.0 - 170.0 MPa | H24 | EN 573-3 | Foil | ||
20.0 °C | 125.0 - 165.0 MPa Show Material materials with Zugfestigkeit of 125.0 - 165.0 MPa | H24 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil | ||
20.0 °C | 125.0 - 165.0 MPa Show Material materials with Zugfestigkeit of 125.0 - 165.0 MPa | H24 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | 20-100°C | |
Schmelzpunkt | 640.0 - 655.0 °C Show Material materials with Schmelzpunkt of 640.0 - 655.0 °C | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | ||
Spezifische Wärmekapazität | 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 920.0 J/(kg·K) | Typical for Wrought 8000 Series Aluminium | ||||
Wärmeleitfähigkeit | 201 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201 W/(m·K) | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | ||
20.0 °C | 210.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 210.0 - 220.0 W/(m·K) | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 34000000.0 - 35000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 34000000.0 - 35000000.0 S/m | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
spezifischer Widerstand | 2.86e-08 - 2.94e-08 Ω·m Show Material materials with spezifischer Widerstand of 2.86e-08 - 2.94e-08 Ω·m | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Strip, Sheet, Plate, Foil | |
3e-08 - 3.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3e-08 - 3.5e-08 Ω·m | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Chrom of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | |
Eisen | 0.5 - 1.0 % Show Material materials with Eisen of 0.5 - 1.0 % | H24 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Coil, Sheet, Strip, Foil, Strip, Plate |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Kupfer of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Magnesium of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Mangan of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | |
Silizium | 0.4 - 0.8 % Show Material materials with Silizium of 0.4 - 0.8 % | H24 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Coil, Sheet, Strip, Foil, Strip, Plate |
Titan | 0.05 % Show Material materials with Titan of 0.05 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.05 % Show Material materials with Titan of 0.05 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil | |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | H24 | EN 573-3, EN 485, EN 541, EN 546, EN 683 | Foil, Sheet, Flat, Strip, Plate |
0.1 % Show Material materials with Zink of 0.1 % | H24 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 546-2, EN 541, EN 683-2 | Coil, Sheet, Strip, Foil |
Technological properties
Property | ||
---|---|---|
Anodizing | Good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Interiors and ceilings: Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins, General applications; Tubes: Flexible tube, Pipes; Insulation; Closures: Long cups, Short cups, Easy open; Cosmetic: Cosmetic pieces; Pharmacy: Pharma and para-pharma; Semi-rigid and corrugated: Pet food, Smooth wall; Foil stock: Foil app | |
Brazing | hard brazing (with flux/ without flux): very good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Moderated | |
Welding | Excellent | |
Workability | Excellent |