Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H111 | EN 573-3 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 180° | 0.5 °/t Show Material materials with Biegewinkel 180° of 0.5 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
1.0 °/t Show Material materials with Biegewinkel 180° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Biegewinkel 90° | 1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Dehnung | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | |
14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A100 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | A50 | ||
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | Transverse | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H111 | EN 573-3 | Flat | ||
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H111 | EN 573-3 | Flat | A50 | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H111 | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Härte, Brinell | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H111 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 25.0 - 27.0 GPa Show Material materials with Schubmodule of 25.0 - 27.0 GPa | H111 | EN 573-3 | Flat | |
Zugfestigkeit | 20.0 °C | 155.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 155.0 - 200.0 MPa | H111 | EN 573-3 | Flat | Transverse |
20.0 °C | 155.0 - 200.0 MPa Show Material materials with Zugfestigkeit of 155.0 - 200.0 MPa | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube |
-50.0 °C | 2.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K | H111 | EN 573-3 | Flat | |
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
20 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
100.0 °C | 2.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K | H111 | EN 573-3 | Flat | |
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
200 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
200.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
300 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
300.0 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube, Flat | |
Schmelzpunkt | 629.0 - 654.0 °C Show Material materials with Schmelzpunkt of 629.0 - 654.0 °C | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
630.0 - 655.0 °C Show Material materials with Schmelzpunkt of 630.0 - 655.0 °C | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H111 | EN 573-3 | Flat | |
Wärmeleitfähigkeit | 160.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 180.0 W/(m·K) | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
163 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 163 W/(m·K) | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 190.0 W/(m·K) | H111 | EN 573-3 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 25000000.0 S/m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 S/m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 24000000.0 S/m | H111 | EN 573-3 | Flat | |
spezifischer Widerstand | 4e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 4.35e-08 Ω·m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.17e-08 Ω·m | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H111 | EN 573-3 | Flat |
0.70 % Show Material materials with Eisen of 0.70 % | H111 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Welded Tube | |
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H111 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Foil, Welded Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |