Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
20.0 °C | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H45 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip |
Abmessung
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 68.6 GPa Show Material materials with Elastizitätsmodul of 68.6 GPa | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Schubmodule | 26.0 GPa Show Material materials with Schubmodule of 26.0 GPa | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
20.0 °C | 25.0 - 27.0 GPa Show Material materials with Schubmodule of 25.0 - 27.0 GPa | H45 | EN 573-3 | Sheet | ||
Streckgrenze | 175.0 - 245.0 MPa Show Material materials with Streckgrenze of 175.0 - 245.0 MPa | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
20.0 °C | 205.0 - 245.0 MPa Show Material materials with Streckgrenze of 205.0 - 245.0 MPa | H45 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube | RP02 | |
Zugfestigkeit | 225.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 225.0 - 270.0 MPa | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 270.0 MPa | H45 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
-50.0 °C | 2.15e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.15e-05 1/K | H45 | EN 573-3 | Sheet | ||
20 °C | 2.1499999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1499999999999997e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100 °C | 2.3199999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3199999999999998e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100.0 °C | 2.32e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.32e-05 1/K | H45 | EN 573-3 | Sheet | ||
100 °C | 2.3899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3899999999999998e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | 20-100°C | |
200 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
200.0 °C | 2.41e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.41e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
300 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
300.0 °C | 2.51e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.51e-05 1/K | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
Schmelzpunkt | 629.0 - 654.0 °C Show Material materials with Schmelzpunkt of 629.0 - 654.0 °C | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
630.0 - 655.0 °C Show Material materials with Schmelzpunkt of 630.0 - 655.0 °C | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |||
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H45 | EN 573-3 | Sheet | ||
Wärmeleitfähigkeit | 160.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 180.0 W/(m·K) | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
163 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 163 W/(m·K) | H45 | EN 573-3, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube, Strip | |||
20.0 °C | 160.0 - 190.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 190.0 W/(m·K) | H45 | EN 573-3 | Sheet |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 25000000.0 S/m | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 24000000.0 S/m | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | ||
20.0 °C | 20000000.0 - 24000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 24000000.0 S/m | H45 | EN 573-3 | Sheet | |
spezifischer Widerstand | 4e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 4.35e-08 Ω·m | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
4.0999999999999997e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.0999999999999997e-08 Ω·m | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | ||
4.17e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.17e-08 Ω·m | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H45 | EN 573-3 | Sheet |
0.70 % Show Material materials with Eisen of 0.70 % | H45 | EN 573-3, EN 541 | Strip, Sheet, Plate, Foil, Welded Tube | |
0.7 % Show Material materials with Eisen of 0.7 % | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Kupfer | 0.25 % Show Material materials with Kupfer of 0.25 % | H45 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Kupfer of 0.25 % | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | H45 | EN 573-3, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube, Strip |
Mangan | 1.0 - 1.5 % Show Material materials with Mangan of 1.0 - 1.5 % | H45 | EN 573-3, EN 541, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube, Strip |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H45 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube |
0.3 % Show Material materials with Silizium of 0.3 % | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip | |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H45 | EN 573-3, EN 541 | Sheet, Strip, Plate, Foil, Welded Tube |
0.25 % Show Material materials with Zink of 0.25 % | H45 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 541 | Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels, Foil for bituminous coating; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Furniture, Plinths, Blinds: Intermediate transformation/interior use; Heat exchangers: Fins; Wind energy: Nacelle coverings, Rotor, Hub, Stairs; Food can: Body, Lids; Semi-rigid and corrugated: Smooth wall | |
Brazing | Very Good | |
Corrosion properties | Seawater: very good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): very good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) very good (H14) / acceptable (H12) |