Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Mechanisch
Property | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|
Elastizitätsmodul | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | |||
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Zugfestigkeit | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Wärmeleitfähigkeit | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Elektrisch
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Elektrische Leitfähigkeit | 22000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 28000000.0 S/m | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
spezifischer Widerstand | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.57e-08 - 4.55e-08 Ω·m | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Mangan | 0.9 - 1.5 % Show Material materials with Mangan of 0.9 - 1.5 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H36 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |