Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 2.73 g/cm³ Show Material materials with Dichte of 2.73 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 65.0 MPa Show Material materials with Bending Fatigue Strength of 65.0 MPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Biegewinkel 180° | 2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
Dehnung | -196.0 °C | 27.0 % Show Material materials with Dehnung of 27.0 % | H14 | EN 573-3 | ||
-80.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | H14 | EN 573-3 | |||
-20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H14 | EN 573-3 | |||
1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 1301 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Wire | A100 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H14 | EN 573-3 | |||
100.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H14 | EN 573-3 | |||
150.0 °C | 16.0 % Show Material materials with Dehnung of 16.0 % | H14 | EN 573-3 | |||
200.0 °C | 20.0 % Show Material materials with Dehnung of 20.0 % | H14 | EN 573-3 | |||
260.0 °C | 60.0 % Show Material materials with Dehnung of 60.0 % | H14 | EN 573-3 | |||
320.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | H14 | EN 573-3 | |||
370.0 °C | 70.0 % Show Material materials with Dehnung of 70.0 % | H14 | EN 573-3 | |||
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |||
20.0 °C | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 - 69.5 GPa Show Material materials with Elastizitätsmodul of 69.0 - 69.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.5 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.5 - 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Härte, Brinell | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 40.0 [-] Show Material materials with Härte, Brinell of 40.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H14 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 24.0 - 26.5 GPa Show Material materials with Schubmodule of 24.0 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 24.0 - 26.1 GPa Show Material materials with Schubmodule of 24.0 - 26.1 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 26.1 - 26.5 GPa Show Material materials with Schubmodule of 26.1 - 26.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | ||
Zugfestigkeit | -196.0 °C | 253.0 MPa Show Material materials with Zugfestigkeit of 253.0 MPa | H14 | EN 573-3 | ||
-80.0 °C | 172.0 MPa Show Material materials with Zugfestigkeit of 172.0 MPa | H14 | EN 573-3 | |||
-20.0 °C | 158.0 MPa Show Material materials with Zugfestigkeit of 158.0 MPa | H14 | EN 573-3 | |||
20.0 °C | 130.0 - 165.0 MPa Show Material materials with Zugfestigkeit of 130.0 - 165.0 MPa | H14 | EN 573-3, EN 754 | Rod, Tube, Strip, Sheet, Plate, Foil, Bar | ||
20.0 °C | 135.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 135.0 - 180.0 MPa | H14 | EN 573-3, EN 1301 | Wire, Strip, Sheet, Plate, Foil, Bar, Rod, Tube | ||
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 140.0 - 180.0 MPa | H14 | EN 573-3, EN 485, EN 683 | Foil, Flat, Strip, Sheet, Plate, Bar, Rod, Tube | ||
20.0 °C | 140.0 - 180.0 MPa Show Material materials with Zugfestigkeit of 140.0 - 180.0 MPa | H14 | EN 573-3 | Flat | Transverse | |
20.0 °C | 155.0 MPa Show Material materials with Zugfestigkeit of 155.0 MPa | H14 | EN 573-3 | |||
100.0 °C | 148.0 MPa Show Material materials with Zugfestigkeit of 148.0 MPa | H14 | EN 573-3 | |||
150.0 °C | 127.0 MPa Show Material materials with Zugfestigkeit of 127.0 MPa | H14 | EN 573-3 | |||
200.0 °C | 98.0 MPa Show Material materials with Zugfestigkeit of 98.0 MPa | H14 | EN 573-3 | |||
260.0 °C | 53.0 MPa Show Material materials with Zugfestigkeit of 53.0 MPa | H14 | EN 573-3 | |||
320.0 °C | 28.0 MPa Show Material materials with Zugfestigkeit of 28.0 MPa | H14 | EN 573-3 | |||
370.0 °C | 19.0 MPa Show Material materials with Zugfestigkeit of 19.0 MPa | H14 | EN 573-3 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube |
100 °C | 2.35e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.35e-05 1/K | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Schmelzpunkt | 645.0 - 655.0 °C Show Material materials with Schmelzpunkt of 645.0 - 655.0 °C | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Spezifische Wärmekapazität | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 892.0 - 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 - 893.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 892.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 892.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 893.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
Wärmeleitfähigkeit | 20.0 °C | 160.0 - 200.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 200.0 W/(m·K) | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
20.0 °C | 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 22000000.0 - 28000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 28000000.0 S/m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube, Flat, Wire |
20.0 °C | 22000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 22000000.0 - 29000000.0 S/m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
spezifischer Widerstand | 3.57e-08 - 4.55e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.57e-08 - 4.55e-08 Ω·m | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
20.0 °C | 3.4e-08 - 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.1e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 3.4e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.5e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 4.1e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire | |
20.0 °C | 4.1e-08 - 4.5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.1e-08 - 4.5e-08 Ω·m | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | H14 | EN 573-3 | Rod, Flat, Foil, Tube, Wire |
0.70 % Show Material materials with Eisen of 0.70 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Foil, Bar, Rod, Tube | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Mangan | 0.9 - 1.5 % Show Material materials with Mangan of 0.9 - 1.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Silizium | 0.5 % Show Material materials with Silizium of 0.5 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H14 | EN 573-3, EN 1301, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Wire, Strip, Sheet, Plate, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): very good to good / very good, friction soldering: very good, soft brazing with flux: very good | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): very good / very good, Impact extrusion (cold): good, Deep drawing / upsetting (Condition) very good (O) / very good (H12) |