Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.72 g/cm³ Show Material materials with Dichte of 2.72 g/cm³ | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Elastizitätsmodul | 69.5 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.5 - 70.0 GPa | Typical for Wrought 3000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 3000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 3000 Series Aluminium | ||||
Schubmodule | 25.0 - 26.0 GPa Show Material materials with Schubmodule of 25.0 - 26.0 GPa | Typical for Wrought 3000 Series Aluminium | ||||
Zugfestigkeit | 20.0 °C | 260.0 - 330.0 MPa Show Material materials with Zugfestigkeit of 260.0 - 330.0 MPa | H19 | EN 573-3 | Sheet | |
20.0 °C | 260.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 260.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 260.0 - 310.0 MPa Show Material materials with Zugfestigkeit of 260.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 - 330.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 330.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 270.0 - 310.0 MPa Show Material materials with Zugfestigkeit of 270.0 - 310.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 290.0 - 330.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 330.0 MPa | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate | ||
20.0 °C | 290.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 300.0 MPa | H19 | EN 573-3 | Sheet | ||
20.0 °C | 290.0 - 310.0 MPa Show Material materials with Zugfestigkeit of 290.0 - 310.0 MPa | H19 | EN 573-3 | Sheet |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.4e-05 1/K | Typical for Wrought 3000 Series Aluminium |
Schmelzpunkt | 629.0 - 654.0 °C Show Material materials with Schmelzpunkt of 629.0 - 654.0 °C | Typical for Wrought 3000 Series Aluminium |
Spezifische Wärmekapazität | 893.0 - 920.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 893.0 - 920.0 J/(kg·K) | Typical for Wrought 3000 Series Aluminium |
Wärmeleitfähigkeit | 154.0 - 193.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 154.0 - 193.0 W/(m·K) | Typical for Wrought 3000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 29000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 29000000.0 S/m | Typical for Wrought 3000 Series Aluminium |
spezifischer Widerstand | 3.4e-08 - 4.2e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.4e-08 - 4.2e-08 Ω·m | Typical for Wrought 3000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Eisen | 0.8 % Show Material materials with Eisen of 0.8 % | H19 | EN 573-3 | Sheet |
0.80 % Show Material materials with Eisen of 0.80 % | H19 | EN 573-3, EN 541 | Strip, Sheet, Plate | |
Gallium | 0.05 % Show Material materials with Gallium of 0.05 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Kupfer | 0.05 - 0.25 % Show Material materials with Kupfer of 0.05 - 0.25 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Magnesium | 0.8 - 1.3 % Show Material materials with Magnesium of 0.8 - 1.3 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Mangan | 0.8 - 1.4 % Show Material materials with Mangan of 0.8 - 1.4 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Silizium | 0.6 % Show Material materials with Silizium of 0.6 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Vanadium | 0.05 % Show Material materials with Vanadium of 0.05 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Zink | 0.25 % Show Material materials with Zink of 0.25 % | H19 | EN 573-3, EN 541 | Sheet, Strip, Plate |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |