Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.66 g/cm³ Show Material materials with Dichte of 2.66 g/cm³ | T64 | EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | T64 | EN 1706, EN 13195 | Casting | ||
Elastizitätsmodul | 20.0 °C | 69.0 - 75.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 75.0 GPa | T64 | EN 1706 | ||
Härte, Brinell | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T64 | EN 1706, EN 13195 | Casting | ||
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T64 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T64 | EN 1706, EN 13195 | Casting | ||
20.0 °C | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T64 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T64 | EN 1706, EN 13195 | Casting | |
100.0 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T64 | EN 1706, EN 13195 | Casting | ||
100 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T64 | EN 1706, EN 13195 | Casting | ||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 150.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 150.0 - 180.0 W/(m·K) | T64 | EN 1706, EN 13195 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 26000000.0 S/m | T64 | EN 1706, EN 13195 | Casting |
spezifischer Widerstand | 3.85e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 5e-08 Ω·m | T64 | EN 1706, EN 13195 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 91.04 % Show Material materials with Aluminium of 91.04 % | T64 | EN 1706 | |
Eisen | 0.19 % Show Material materials with Eisen of 0.19 % | T64 | EN 1706 | |
0.19 % Show Material materials with Eisen of 0.19 % | T64 | EN 1706, EN 13195 | Casting | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | T64 | EN 1706, EN 13195 | Casting |
Magnesium | 0.45 - 0.7 % Show Material materials with Magnesium of 0.45 - 0.7 % | T64 | EN 1706, EN 13195 | Casting |
Mangan | 0.1 % Show Material materials with Mangan of 0.1 % | T64 | EN 1706, EN 13195 | Casting |
Silizium | 6.5 - 7.5 % Show Material materials with Silizium of 6.5 - 7.5 % | T64 | EN 1706, EN 13195 | Casting |
Titan | 0.08 - 0.25 % Show Material materials with Titan of 0.08 - 0.25 % | T64 | EN 1706, EN 13195 | Casting |
Zink | 0.07 % Show Material materials with Zink of 0.07 % | T64 | EN 1706, EN 13195 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not sufficient | |
Corrosion properties | general: good | |
General machinability | as cast: good | |
Processing methods | permanent mould casting, separately cast test sample |