Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.65 g/cm³ Show Material materials with Dichte of 2.65 g/cm³ | F | EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | Casting | ||
Elastizitätsmodul | 71.0 - 75.0 GPa Show Material materials with Elastizitätsmodul of 71.0 - 75.0 GPa | Typical for Cast 4xx.x Series Aluminium | ||||
Härte, Brinell | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | F | EN 1706 | Casting | ||
55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | EN 1706 | Casting | |||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | F | EN 1706 | |||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | ||||
Zugfestigkeit | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706 | Casting | ||
170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 | Casting | |||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706 | |||
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | F | EN 1706 | Casting | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | F | EN 1706 | Casting | ||
100.0 °C | 2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2e-05 1/K | F | EN 1706 | |||
Schmelzpunkt | 565.0 - 630.0 °C Show Material materials with Schmelzpunkt of 565.0 - 630.0 °C | Typical for Cast 4xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 963.0 J/(kg·K) | Typical for Cast 4xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 160.0 W/(m·K) | F | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 16000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 23000000.0 S/m | F | EN 1706 | Casting |
spezifischer Widerstand | 4.35e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 6.25e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 84.35 % Show Material materials with Aluminium of 84.35 % | F | EN 1706 | |
Blei | 0.1 % Show Material materials with Blei of 0.1 % | F | EN 1706 | Casting |
Eisen | 0.65 % Show Material materials with Eisen of 0.65 % | F | EN 1706 | |
0.65 % Show Material materials with Eisen of 0.65 % | F | EN 1706 | Casting | |
Kupfer | 0.15 % Show Material materials with Kupfer of 0.15 % | F | EN 1706 | Casting |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | F | EN 1706 | Casting |
Mangan | 0.55 % Show Material materials with Mangan of 0.55 % | F | EN 1706 | Casting |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | F | EN 1706 | Casting |
Silizium | 10.5 - 13.5 % Show Material materials with Silizium of 10.5 - 13.5 % | F | EN 1706 | Casting |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | F | EN 1706 | Casting |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: good to acceptable | |
General machinability | after thermal treatment: acceptable | |
Processing methods | investment casting, separately cast test sample |