Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.71 g/cm³ Show Material materials with Dichte of 2.65 - 2.71 g/cm³ | Typical for Cast 4xx.x Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | Casting | ||
Elastizitätsmodul | 74.0 GPa Show Material materials with Elastizitätsmodul of 74.0 GPa | F | EN 1706 | Casting | ||
Härte, Brinell | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | EN 1706 | Casting | ||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | F | EN 1706 | |||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 4xx.x Series Aluminium | ||||
Zugfestigkeit | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | F | EN 1706 | Casting | ||
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 | |||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | F | EN 1706 | |||
20.0 °C | 220.0 MPa Show Material materials with Zugfestigkeit of 220.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting |
20 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | F | EN 1706 | Casting | |
100.0 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting | |
100 °C | 2.1e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.1e-05 1/K | F | EN 1706 | Casting | |
200 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | F | EN 1706 | Casting | |
Schmelzpunkt | 550.0 - 600.0 °C Show Material materials with Schmelzpunkt of 550.0 - 600.0 °C | F | EN 1706 | Casting | |
Spezifische Wärmekapazität | 910.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 910.0 J/(kg·K) | F | EN 1706 | Casting | |
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 150.0 W/(m·K) | F | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 16000000.0 - 22000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 22000000.0 S/m | F | EN 1706 | Casting |
spezifischer Widerstand | 4.55e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.55e-08 - 6.25e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 87.05 % Show Material materials with Aluminium of 87.05 % | F | EN 1706 | |
Blei | 0.05 % Show Material materials with Blei of 0.05 % | F | EN 1706 | Casting |
Eisen | 0.65 % Show Material materials with Eisen of 0.65 % | F | EN 1706 | |
0.65 % Show Material materials with Eisen of 0.65 % | F | EN 1706 | Casting | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | F | EN 1706 | Casting |
Magnesium | 0.1 % Show Material materials with Magnesium of 0.1 % | F | EN 1706 | Casting |
Mangan | 0.5 % Show Material materials with Mangan of 0.5 % | F | EN 1706 | Casting |
Nickel | 0.05 % Show Material materials with Nickel of 0.05 % | F | EN 1706 | Casting |
Silizium | 8.0 - 11.0 % Show Material materials with Silizium of 8.0 - 11.0 % | F | EN 1706 | Casting |
Titan | 0.15 % Show Material materials with Titan of 0.15 % | F | EN 1706 | Casting |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | F | EN 1706 | Casting |
Zinn | 0.05 % Show Material materials with Zinn of 0.05 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: acceptable | |
General machinability | after thermal treatment: acceptable | |
Processing methods | permanent mould casting, separately cast test sample |