Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.7 g/cm³ Show Material materials with Dichte of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 70.0 - 100.0 MPa Show Material materials with Bending Fatigue Strength of 70.0 - 100.0 MPa | T4 | EN 1706 | Casting | ||
Elastizitätsmodul | 73.0 - 80.0 GPa Show Material materials with Elastizitätsmodul of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Härte, Brinell | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T4 | EN 1706 | Casting | ||
85.0 [-] Show Material materials with Härte, Brinell of 85.0 [-] | T4 | EN 1706 | Casting | |||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | T4 | EN 1706 | |||
20.0 °C | 85.0 [-] Show Material materials with Härte, Brinell of 85.0 [-] | T4 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T4 | EN 1706 | Casting | ||
230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | EN 1706 | Casting | |||
20.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | T4 | EN 1706 | |||
20.0 °C | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | |
100.0 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | ||
100 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | ||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 150.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 150.0 W/(m·K) | T4 | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 19000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 19000000.0 - 23000000.0 S/m | T4 | EN 1706 | Casting |
spezifischer Widerstand | 4.35e-08 - 5.26e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 5.26e-08 Ω·m | T4 | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 90.15 % Show Material materials with Aluminium of 90.15 % | T4 | EN 1706 | |
Blei | 0.15 % Show Material materials with Blei of 0.15 % | T4 | EN 1706 | Casting |
Eisen | 0.65 % Show Material materials with Eisen of 0.65 % | T4 | EN 1706 | |
0.65 % Show Material materials with Eisen of 0.65 % | T4 | EN 1706 | Casting | |
Kupfer | 1.0 - 1.5 % Show Material materials with Kupfer of 1.0 - 1.5 % | T4 | EN 1706 | Casting |
Magnesium | 0.35 - 0.65 % Show Material materials with Magnesium of 0.35 - 0.65 % | T4 | EN 1706 | Casting |
Mangan | 0.55 % Show Material materials with Mangan of 0.55 % | T4 | EN 1706 | Casting |
Nickel | 0.25 % Show Material materials with Nickel of 0.25 % | T4 | EN 1706 | Casting |
Silizium | 4.5 - 5.5 % Show Material materials with Silizium of 4.5 - 5.5 % | T4 | EN 1706 | Casting |
Titan | 0.05 - 0.25 % Show Material materials with Titan of 0.05 - 0.25 % | T4 | EN 1706 | Casting |
Zink | 0.15 % Show Material materials with Zink of 0.15 % | T4 | EN 1706 | Casting |
Zinn | 0.05 % Show Material materials with Zinn of 0.05 % | T4 | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not sufficient | |
Corrosion properties | general: not sufficient | |
General machinability | after thermal treatment: good, as cast: good | |
Processing methods | permanent mould casting, separately cast test sample |