Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.7 g/cm³ Show Material materials with Dichte of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 70.0 - 100.0 MPa Show Material materials with Bending Fatigue Strength of 70.0 - 100.0 MPa | T4 | EN 1706 | Casting | ||
Elastizitätsmodul | 73.0 - 80.0 GPa Show Material materials with Elastizitätsmodul of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Härte, Brinell | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T4 | EN 1706 | Casting | ||
20.0 °C | 75.0 [-] Show Material materials with Härte, Brinell of 75.0 [-] | T4 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | EN 1706 | Casting | ||
20.0 °C | 230.0 MPa Show Material materials with Zugfestigkeit of 230.0 MPa | T4 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | |
100.0 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | ||
100 °C | 2.2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 1/K | T4 | EN 1706 | Casting | ||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 120.0 - 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 130.0 W/(m·K) | T4 | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 16000000.0 - 19000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 16000000.0 - 19000000.0 S/m | T4 | EN 1706 | Casting |
spezifischer Widerstand | 5.26e-08 - 6.25e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.26e-08 - 6.25e-08 Ω·m | T4 | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 88.35 % Show Material materials with Aluminium of 88.35 % | T4 | EN 1706 | |
Blei | 0.1 % Show Material materials with Blei of 0.1 % | T4 | EN 1706 | Casting |
Eisen | 0.6 % Show Material materials with Eisen of 0.6 % | T4 | EN 1706 | |
0.60 % Show Material materials with Eisen of 0.60 % | T4 | EN 1706 | Casting | |
Kupfer | 2.6 - 3.6 % Show Material materials with Kupfer of 2.6 - 3.6 % | T4 | EN 1706 | Casting |
Magnesium | 0.05 % Show Material materials with Magnesium of 0.05 % | T4 | EN 1706 | Casting |
Mangan | 0.55 % Show Material materials with Mangan of 0.55 % | T4 | EN 1706 | Casting |
Nickel | 0.1 % Show Material materials with Nickel of 0.1 % | T4 | EN 1706 | Casting |
Silizium | 4.5 - 6.0 % Show Material materials with Silizium of 4.5 - 6.0 % | T4 | EN 1706 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T4 | EN 1706 | Casting |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | T4 | EN 1706 | Casting |
Zinn | 0.05 % Show Material materials with Zinn of 0.05 % | T4 | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not sufficient | |
Corrosion properties | general: not sufficient | |
General machinability | after thermal treatment: good, as cast: good | |
Processing methods | permanent mould casting, separately cast test sample |