Allgemein
Property | Value | Comment |
---|---|---|
Dichte | 2.65 - 2.7 g/cm³ Show Material materials with Dichte of 2.65 - 2.7 g/cm³ | Typical for Cast 3xx.x Series Aluminium |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706 | Casting | ||
Elastizitätsmodul | 73.0 - 80.0 GPa Show Material materials with Elastizitätsmodul of 73.0 - 80.0 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Härte, Brinell | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | F | EN 1706 | Casting | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | F | EN 1706 | Casting | ||
20.0 °C | 240.0 MPa Show Material materials with Zugfestigkeit of 240.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | F | EN 1706 | Casting | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | F | EN 1706 | Casting | ||
100.0 °C | 2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2e-05 1/K | F | EN 1706 | |||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 120.0 - 130.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 120.0 - 130.0 W/(m·K) | F | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 14000000.0 - 18000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 14000000.0 - 18000000.0 S/m | F | EN 1706 | Casting |
spezifischer Widerstand | 5.56e-08 - 7.14e-08 Ω·m Show Material materials with spezifischer Widerstand of 5.56e-08 - 7.14e-08 Ω·m | F | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 80.25 % Show Material materials with Aluminium of 80.25 % | F | EN 1706 | |
Blei | 0.25 % Show Material materials with Blei of 0.25 % | F | EN 1706 | Casting |
Chrom | 0.15 % Show Material materials with Chrom of 0.15 % | F | EN 1706 | Casting |
Eisen | 1.1 % Show Material materials with Eisen of 1.1 % | F | EN 1706 | |
1.10 % Show Material materials with Eisen of 1.10 % | F | EN 1706 | Casting | |
Kupfer | 1.5 - 2.5 % Show Material materials with Kupfer of 1.5 - 2.5 % | F | EN 1706 | Casting |
Magnesium | 0.3 % Show Material materials with Magnesium of 0.3 % | F | EN 1706 | Casting |
Mangan | 0.55 % Show Material materials with Mangan of 0.55 % | F | EN 1706 | Casting |
Nickel | 0.45 % Show Material materials with Nickel of 0.45 % | F | EN 1706 | Casting |
Silizium | 10.0 - 12.0 % Show Material materials with Silizium of 10.0 - 12.0 % | F | EN 1706 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | F | EN 1706 | Casting |
Zink | 1.7 % Show Material materials with Zink of 1.7 % | F | EN 1706 | Casting |
Zinn | 0.25 % Show Material materials with Zinn of 0.25 % | F | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: not sufficient | |
General machinability | after thermal treatment: acceptable | |
Processing methods | pressure die casting, separately cast test sample |