Allgemein
Property | Temperature | Value | Condition | Related Standards |
---|---|---|---|---|
Dichte | 20.0 °C | 2.68 g/cm³ Show Material materials with Dichte of 2.68 g/cm³ | T5 | EN 1706 |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 - 110.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 - 110.0 MPa | T5 | EN 1706 | Casting | ||
Elastizitätsmodul | 20.0 °C | 77.0 - 83.0 GPa Show Material materials with Elastizitätsmodul of 77.0 - 83.0 GPa | T5 | EN 1706 | ||
Härte, Brinell | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T5 | EN 1706 | Casting | ||
20.0 °C | 90.0 [-] Show Material materials with Härte, Brinell of 90.0 [-] | T5 | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 3xx.x Series Aluminium | ||||
Schubmodule | 2.8 GPa Show Material materials with Schubmodule of 2.8 GPa | Typical for Cast 3xx.x Series Aluminium | ||||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T5 | EN 1706 | Casting | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | T5 | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | T5 | EN 1706 | Casting | |
100 °C | 1.9999999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 1.9999999999999998e-05 1/K | T5 | EN 1706 | Casting | ||
100.0 °C | 2e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2e-05 1/K | T5 | EN 1706 | |||
Schmelzpunkt | 505.0 - 770.0 °C Show Material materials with Schmelzpunkt of 505.0 - 770.0 °C | Typical for Cast 3xx.x Series Aluminium | ||||
Spezifische Wärmekapazität | 960.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 960.0 - 963.0 J/(kg·K) | Typical for Cast 3xx.x Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 160.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 160.0 W/(m·K) | T5 | EN 1706 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 15000000.0 - 23000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 15000000.0 - 23000000.0 S/m | T5 | EN 1706 | Casting |
spezifischer Widerstand | 4.35e-08 - 6.67e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.35e-08 - 6.67e-08 Ω·m | T5 | EN 1706 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 80.4 % Show Material materials with Aluminium of 80.4 % | T5 | EN 1706 | |
Eisen | 0.7 % Show Material materials with Eisen of 0.7 % | T5 | EN 1706 | |
0.70 % Show Material materials with Eisen of 0.70 % | T5 | EN 1706 | Casting | |
Kupfer | 0.8 - 1.5 % Show Material materials with Kupfer of 0.8 - 1.5 % | T5 | EN 1706 | Casting |
Magnesium | 0.8 - 1.5 % Show Material materials with Magnesium of 0.8 - 1.5 % | T5 | EN 1706 | Casting |
Mangan | 0.35 % Show Material materials with Mangan of 0.35 % | T5 | EN 1706 | Casting |
Nickel | 0.7 - 1.3 % Show Material materials with Nickel of 0.7 - 1.3 % | T5 | EN 1706 | Casting |
Silizium | 10.5 - 13.5 % Show Material materials with Silizium of 10.5 - 13.5 % | T5 | EN 1706 | Casting |
Titan | 0.25 % Show Material materials with Titan of 0.25 % | T5 | EN 1706 | Casting |
Zink | 0.35 % Show Material materials with Zink of 0.35 % | T5 | EN 1706 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: not recommended | |
Corrosion properties | general: acceptable | |
General machinability | as cast: good | |
Processing methods | permanent mould casting, separately cast test sample |