Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | H28 | EN 573-3 | Flat | |
20.0 °C | 2.69 - 2.7 g/cm³ Show Material materials with Dichte of 2.69 - 2.7 g/cm³ | H28 | EN 573-3 | Flat | |
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H28 | EN 573-3 | Flat |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Biegewinkel 90° | 1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |||
Elastizitätsmodul | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H28 | EN 573-3 | Flat | ||
Härte, Brinell | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H28 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H28 | EN 573-3 | Flat | |
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 25.0 - 26.1 GPa Show Material materials with Schubmodule of 25.0 - 26.1 GPa | H28 | EN 573-3 | Flat | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H28 | EN 573-3 | Flat | ||
Zugfestigkeit | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
20.0 °C | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H28 | EN 573-3 | Flat | Transverse | |
20.0 °C | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H28 | EN 573-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | -50 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | |
-50.0 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
20 °C | 2.18e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.18e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
20 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
20 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
20 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
100 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
100.0 °C | 2.36e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.36e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
200 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
200.0 °C | 2.45e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.45e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
300 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
300.0 °C | 2.55e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.55e-05 1/K | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 630.0 - 650.0 °C Show Material materials with Schmelzpunkt of 630.0 - 650.0 °C | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 879.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 J/(kg·K) | H28 | EN 573-3 | Flat | |
20.0 °C | 879.0 - 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 899.0 J/(kg·K) | H28 | EN 573-3 | Flat | ||
20.0 °C | 899.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 899.0 J/(kg·K) | H28 | EN 573-3 | Flat | ||
Wärmeleitfähigkeit | 20.0 °C | 160.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 220.0 W/(m·K) | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar, Flat | |
20.0 °C | 160.0 - 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 160.0 - 201.0 W/(m·K) | H28 | EN 573-3 | Flat | ||
20.0 °C | 201.0 - 220.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 - 220.0 W/(m·K) | H28 | EN 573-3 | Flat | ||
20.0 °C | 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 W/(m·K) | H28 | EN 573-3 | Flat |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 23000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 31000000.0 S/m | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
spezifischer Widerstand | 3.23e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.23e-08 - 4.35e-08 Ω·m | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 Ω·m | H28 | EN 573-3 | Flat |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Eisen | 0.45 % Show Material materials with Eisen of 0.45 % | H28 | EN 573-3 | Flat |
0.45 % Show Material materials with Eisen of 0.45 % | H28 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Bar | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Magnesium | 0.7 - 1.1 % Show Material materials with Magnesium of 0.7 - 1.1 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H28 | EN 573-3, EN 485 | Flat, Strip, Sheet, Plate, Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: gut (EQ: sehr gut), Protective: very good | |
Brazing | hard brazing (with flux/ without flux): sufficient - poor / sufficient, friction soldering: good, soft brazing with flux: acceptable | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (H12) |