Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 80.0 MPa Show Material materials with Bending Fatigue Strength of 80.0 MPa | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Biegewinkel 90° | 1.5 °/t Show Material materials with Biegewinkel 90° of 1.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
3.0 °/t Show Material materials with Biegewinkel 90° of 3.0 °/t | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Dehnung | 0.5 % Show Material materials with Dehnung of 0.5 % | H18 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | |
1.0 % Show Material materials with Dehnung of 1.0 % | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H18 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H18 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 0.5 % Show Material materials with Dehnung of 0.5 % | H18 | EN 573-3 | Foil | A50 | |
20.0 °C | 0.5 % Show Material materials with Dehnung of 0.5 % | H18 | EN 573-3 | Foil | A100 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H18 | EN 573-3 | Flat | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H18 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H18 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H18 | EN 573-3 | Seamless Tube | ||
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H18 | EN 573-3 | Rod, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
Härte, Brinell | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H18 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 55.0 [-] Show Material materials with Härte, Brinell of 55.0 [-] | H18 | EN 573-3 | Rod, Tube | ||
20.0 °C | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H18 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | ||
Zugfestigkeit | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H18 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H18 | EN 573-3, EN 1592 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H18 | EN 573-3 | Rod, Foil, Tube, Flat | ||
20.0 °C | 185.0 MPa Show Material materials with Zugfestigkeit of 185.0 MPa | H18 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H18 | EN 573-3 | Seamless Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 630.0 - 655.0 °C Show Material materials with Schmelzpunkt of 630.0 - 655.0 °C | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
Wärmeleitfähigkeit | 201 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201 W/(m·K) | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 W/(m·K) | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 30000000.0 S/m | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
spezifischer Widerstand | 3.33e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 Ω·m | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 Ω·m | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Eisen | 0.45 % Show Material materials with Eisen of 0.45 % | H18 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Eisen of 0.7 % | H18 | EN 573-3 | Rod, Flat, Foil, Seamless Tube, Tube | |
0.70 % Show Material materials with Eisen of 0.70 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H18 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Kupfer of 0.2 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
Magnesium | 0.5 - 1.1 % Show Material materials with Magnesium of 0.5 - 1.1 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.7 - 1.1 % Show Material materials with Magnesium of 0.7 - 1.1 % | H18 | EN 573-3 | Rod, Tube | |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | H18 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Mangan of 0.2 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H18 | EN 573-3 | Rod, Tube |
0.25 % Show Material materials with Zink of 0.25 % | H18 | EN 573-3, EN 1592, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Seamless Tube, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Brazing | hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O) |