Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
20.0 °C | 2.7 g/cm³ Show Material materials with Dichte of 2.7 g/cm³ | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Abmessung
Property | Value | Condition | Related Standards | Thickness | Shape |
---|---|---|---|---|---|
Dicke | 0.2 mm Show Material materials with Dicke of 0.2 mm | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 0.2 mm | Coil, Sheet, Strip |
3.0 mm Show Material materials with Dicke of 3.0 mm | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | 3.0 mm | Coil, Sheet, Strip |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 75.0 MPa Show Material materials with Bending Fatigue Strength of 75.0 MPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Biegewinkel 180° | 1.5 °/t Show Material materials with Biegewinkel 180° of 1.5 °/t | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
2.0 °/t Show Material materials with Biegewinkel 180° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 180° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Biegewinkel 90° | 0.5 °/t Show Material materials with Biegewinkel 90° of 0.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
1.0 °/t Show Material materials with Biegewinkel 90° of 1.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
1 °/t Show Material materials with Biegewinkel 90° of 1 °/t | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
2.0 °/t Show Material materials with Biegewinkel 90° of 2.0 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
2.5 °/t Show Material materials with Biegewinkel 90° of 2.5 °/t | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
Dehnung | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | |
2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
2.0 - 3.0 % Show Material materials with Dehnung of 2.0 - 3.0 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | A50 | ||
3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3, EN 485, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A50 | ||
6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | A100 | ||
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A50 | |
20.0 °C | 1.0 % Show Material materials with Dehnung of 1.0 % | H14 | EN 573-3 | Foil | A100 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Rod, Tube, Flat | A50 | |
20.0 °C | 4.0 % Show Material materials with Dehnung of 4.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 | |
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | H14 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | H14 | EN 573-3 | Rod, Tube | ||
Elastizitätsmodul | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 69.5 GPa Show Material materials with Elastizitätsmodul of 69.5 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Härte, Brinell | 48.0 [-] Show Material materials with Härte, Brinell of 48.0 [-] | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 45.0 [-] Show Material materials with Härte, Brinell of 45.0 [-] | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 48.0 [-] Show Material materials with Härte, Brinell of 48.0 [-] | H14 | EN 573-3 | Flat | ||
Härte, HBW | 48 [-] Show Material materials with Härte, HBW of 48 [-] | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 20.0 °C | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Schubmodule | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
26.5 GPa Show Material materials with Schubmodule of 26.5 GPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
20.0 °C | 26.1 GPa Show Material materials with Schubmodule of 26.1 GPa | H14 | EN 573-3 | Rod, Flat, Foil, Tube | ||
Streckgrenze | 110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | |
120.0 MPa Show Material materials with Streckgrenze of 120.0 MPa | H14 | EN 573-3, EN 485 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
120 MPa Show Material materials with Streckgrenze of 120 MPa | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |||
125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | H14 | EN 573-3, EN 683 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | RP02 | ||
20.0 °C | 110.0 MPa Show Material materials with Streckgrenze of 110.0 MPa | H14 | EN 573-3 | Rod, Tube | RP02 | |
20.0 °C | 120.0 MPa Show Material materials with Streckgrenze of 120.0 MPa | H14 | EN 573-3 | Flat | RP02 | |
20.0 °C | 120.0 MPa Show Material materials with Streckgrenze of 120.0 MPa | H14 | EN 573-3 | Flat | RP02 Transverse | |
20.0 °C | 125.0 MPa Show Material materials with Streckgrenze of 125.0 MPa | H14 | EN 573-3 | Foil | RP02 | |
Zugfestigkeit | 140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | H14 | EN 573-3, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | H14 | EN 573-3 | Rod, Tube | ||
20.0 °C | 145.0 - 190.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 190.0 MPa | H14 | EN 573-3, EN 683 | Foil, Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 185.0 MPa | H14 | EN 573-3, EN 485, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Flat, Strip, Sheet, Plate, Tube, Welded Tube, Bar, Coil, Sheet, Strip | ||
20.0 °C | 145.0 - 185.0 MPa Show Material materials with Zugfestigkeit of 145.0 - 185.0 MPa | H14 | EN 573-3 | Flat | Transverse |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
100 °C | 2.38e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.38e-05 1/K | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
100 °C | 0.000024 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 0.000024 1/K | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | 20-100°C | |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | ||||
Schmelzpunkt | 630.0 - 655.0 °C Show Material materials with Schmelzpunkt of 630.0 - 655.0 °C | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | ||
Spezifische Wärmekapazität | 20.0 °C | 897.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 897.0 J/(kg·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
Wärmeleitfähigkeit | 200 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 200 W/(m·K) | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | ||
201 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201 W/(m·K) | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |||
20.0 °C | 201.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 201.0 W/(m·K) | H14 | EN 573-3 | Rod, Flat, Foil, Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 30000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 30000000.0 S/m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
spezifischer Widerstand | 3.33e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.33e-08 Ω·m | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
20.0 °C | 3.3e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 Ω·m | H14 | EN 573-3, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Rod, Flat, Foil, Tube, Coil, Sheet, Strip |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.1 % Show Material materials with Chrom of 0.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.1 % Show Material materials with Chrom of 0.1 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Eisen | 0.45 % Show Material materials with Eisen of 0.45 % | H14 | EN 573-3 | Rod, Tube |
0.7 % Show Material materials with Eisen of 0.7 % | H14 | EN 573-3 | Rod, Flat, Foil, Tube | |
0.70 % Show Material materials with Eisen of 0.70 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Strip, Sheet, Plate, Tube, Welded Tube, Bar | |
0.7 % Show Material materials with Eisen of 0.7 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | H14 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Kupfer of 0.2 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Kupfer of 0.2 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Magnesium | 0.5 - 1.1 % Show Material materials with Magnesium of 0.5 - 1.1 % | H14 | EN 573-3, EN 485, EN 683, EN 754, EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar, Coil, Sheet, Strip |
0.7 - 1.1 % Show Material materials with Magnesium of 0.7 - 1.1 % | H14 | EN 573-3 | Rod, Tube | |
Mangan | 0.15 % Show Material materials with Mangan of 0.15 % | H14 | EN 573-3 | Rod, Tube |
0.2 % Show Material materials with Mangan of 0.2 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.2 % Show Material materials with Mangan of 0.2 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Silizium | 0.3 % Show Material materials with Silizium of 0.3 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar |
0.3 % Show Material materials with Silizium of 0.3 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip | |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H14 | EN 573-3 | Rod, Tube |
0.25 % Show Material materials with Zink of 0.25 % | H14 | EN 573-3, EN 485, EN 683, EN 754 | Rod, Flat, Foil, Tube, Strip, Sheet, Plate, Welded Tube, Bar | |
0.25 % Show Material materials with Zink of 0.25 % | H14 | EN 573-1, EN 573-2, EN 573-3, EN 485-2, EN 683-2 | Coil, Sheet, Strip |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: acceptable, Protective: very good | |
Application areas | Facades: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Roofing: Single sheet, Sheets for composites/ sandwich Panels; Doors: Sheets for composites/ sandwich Panels, Sheets for mechanized panels; Sun Protection Systems: Single sheet (covering, sun breakers and gutters); Interiors and ceilings: Single sheet, Sheets for composites/ sandwich Panels, Sheets for mechanized panels, Decoration; Furniture, Plinths, Blinds: Single sheet, Intermediate transformation/interior use; Anodizing quality; Heat exchangers: Fins, General applications; Cosmetics: Cosmetics pieces; Automotive trim: Interior trim; Components: Automotive fins, Heat exchangers | |
Brazing | hard brazing (with flux/ without flux): acceptable / sufficient, friction soldering: good, soft brazing with flux: sufficient | |
Corrosion properties | Seawater: good, weathering: very good | |
Welding | Very Good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): acceptable, Deep drawing / upsetting (Condition) good (O) / good (O) |