Allgemein
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Dichte | 2.69 g/cm³ Show Material materials with Dichte of 2.69 g/cm³ | O | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 5.0 % Show Material materials with Dehnung of 5.0 % | O | EN 573-3, EN 1386 | Strip, Sheet, Plate | A50 | |
6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3, EN 1386, EN 485 | Strip, Sheet, Plate | A100 | ||
9.0 % Show Material materials with Dehnung of 9.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
11.0 % Show Material materials with Dehnung of 11.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate | A100 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3, EN 485 | Strip, Sheet, Plate | A50 | ||
20.0 °C | 5.0 % Show Material materials with Dehnung of 5.0 % | O | EN 573-3 | Plate | A50 | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 6.0 % Show Material materials with Dehnung of 6.0 % | O | EN 573-3 | Plate, Sheet | ||
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 9.0 % Show Material materials with Dehnung of 9.0 % | O | EN 573-3 | Sheet | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | O | EN 573-3 | Sheet | ||
20.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | O | EN 573-3 | Flat | Transverse | |
20.0 °C | 11.0 % Show Material materials with Dehnung of 11.0 % | O | EN 573-3 | Flat | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | O | EN 573-3 | Flat | A50 | |
Elastizitätsmodul | 69.0 - 70.0 GPa Show Material materials with Elastizitätsmodul of 69.0 - 70.0 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 26.0 - 26.5 GPa Show Material materials with Schubmodule of 26.0 - 26.5 GPa | Typical for Wrought 5000 Series Aluminium | ||||
Zugfestigkeit | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | O | EN 573-3, EN 1386 | Strip, Sheet, Plate | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | O | EN 573-3 | Plate | ||
20.0 °C | 210.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 300.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 210.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 285.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 210.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 270.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 210.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 270.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 210.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 300.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 210.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 210.0 - 285.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 230.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 300.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 230.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 285.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 270.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 230.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 285.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate | ||
20.0 °C | 230.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 300.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 230.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 230.0 - 270.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 245.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 300.0 MPa | O | EN 573-3 | Sheet, Flat | Transverse | |
20.0 °C | 245.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 285.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 245.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 270.0 MPa | O | EN 573-3 | Sheet | Transverse | |
20.0 °C | 245.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 300.0 MPa | O | EN 573-3, EN 485 | Strip, Sheet, Plate, Flat | ||
20.0 °C | 245.0 - 285.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 285.0 MPa | O | EN 573-3 | Sheet | ||
20.0 °C | 245.0 - 270.0 MPa Show Material materials with Zugfestigkeit of 245.0 - 270.0 MPa | O | EN 573-3 | Sheet |
Thermisch
Property | Value | Comment |
---|---|---|
Koeffizient der thermischen Ausdehnung | 2.2e-05 - 2.5e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2e-05 - 2.5e-05 1/K | Typical for Wrought 5000 Series Aluminium |
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium |
Schmelzpunkt | 560.0 - 655.0 °C Show Material materials with Schmelzpunkt of 560.0 - 655.0 °C | Typical for Wrought 5000 Series Aluminium |
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium |
Wärmeleitfähigkeit | 112.0 - 205.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 112.0 - 205.0 W/(m·K) | Typical for Wrought 5000 Series Aluminium |
Elektrisch
Property | Value | Comment |
---|---|---|
Elektrische Leitfähigkeit | 18000000.0 - 31000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 18000000.0 - 31000000.0 S/m | Typical for Wrought 5000 Series Aluminium |
spezifischer Widerstand | 3.3e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.3e-08 - 5e-08 Ω·m | Typical for Wrought 5000 Series Aluminium |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Eisen | 0.2 - 1.0 % Show Material materials with Eisen of 0.2 - 1.0 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Kupfer | 0.1 - 0.8 % Show Material materials with Kupfer of 0.1 - 0.8 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Magnesium | 3.9 - 4.9 % Show Material materials with Magnesium of 3.9 - 4.9 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Mangan | 0.6 - 1.8 % Show Material materials with Mangan of 0.6 - 1.8 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Silizium | 0.55 - 1.4 % Show Material materials with Silizium of 0.55 - 1.4 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Zink | 1.0 % Show Material materials with Zink of 1.0 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Zirkonium | 0.3 % Show Material materials with Zirkonium of 0.3 % | O | EN 573-3, EN 1386, EN 485 | Sheet, Flat, Plate, Strip |
Technological properties
Property | ||
---|---|---|
Workability | Good workability. |