Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 10.0 % Show Material materials with Dehnung of 10.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | |
12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
13.0 % Show Material materials with Dehnung of 13.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | ||
14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
15.0 % Show Material materials with Dehnung of 15.0 % | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H112 | EN 573-3 | Flat | ||
20.0 °C | 10.0 % Show Material materials with Dehnung of 10.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3 | Flat | A50 Transverse | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3 | Flat | A50 | |
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3 | Sheet | ||
20.0 °C | 12.0 % Show Material materials with Dehnung of 12.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 13.0 % Show Material materials with Dehnung of 13.0 % | H112 | EN 573-3 | Profile, Rod, Tube | A50 | |
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3 | A50 Transverse | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3 | Rod, Sheet, Tube, Profile | ||
20.0 °C | 14.0 % Show Material materials with Dehnung of 14.0 % | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 15.0 % Show Material materials with Dehnung of 15.0 % | H112 | EN 573-3 | Rod, Tube, Profile | ||
Elastizitätsmodul | -270 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | |
-270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | ||
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | ||
300 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube, Profile, Flat | ||
Härte, Brinell | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
62.0 [-] Show Material materials with Härte, Brinell of 62.0 [-] | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | H112 | EN 573-3 | Profile, Rod, Tube | ||
20.0 °C | 52.0 [-] Show Material materials with Härte, Brinell of 52.0 [-] | H112 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 52.0 - 62.0 [-] Show Material materials with Härte, Brinell of 52.0 - 62.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 52.0 - 58.0 [-] Show Material materials with Härte, Brinell of 52.0 - 58.0 [-] | H112 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 58.0 - 62.0 [-] Show Material materials with Härte, Brinell of 58.0 - 62.0 [-] | H112 | EN 573-3 | Flat | ||
20.0 °C | 58.0 [-] Show Material materials with Härte, Brinell of 58.0 [-] | H112 | EN 573-3 | Flat, Sheet | ||
20.0 °C | 62.0 [-] Show Material materials with Härte, Brinell of 62.0 [-] | H112 | EN 573-3 | Flat | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schlagfestigkeit, Charpy gekerbt | 30.0 kJ/m² Show Material materials with Schlagfestigkeit, Charpy gekerbt of 30.0 kJ/m² | H112 | EN 573-3 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Schubmodule | 20.0 °C | 26.5 Show Material materials with Schubmodule of 26.5 | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | |
Zugfestigkeit | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H112 | EN 573-3, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H112 | EN 573-3, EN 485 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 180.0 MPa Show Material materials with Zugfestigkeit of 180.0 MPa | H112 | EN 573-3 | Rod, Tube, Profile | ||
20.0 °C | 190.0 - 240.0 MPa Show Material materials with Zugfestigkeit of 190.0 - 240.0 MPa | H112 | EN 573-3 | Transverse | ||
20.0 °C | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 190.0 MPa Show Material materials with Zugfestigkeit of 190.0 MPa | H112 | EN 573-3 | Sheet | ||
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 200.0 MPa Show Material materials with Zugfestigkeit of 200.0 MPa | H112 | EN 573-3 | Rod, Tube, Profile, Flat | ||
20.0 °C | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H112 | EN 573-3 | Flat | Transverse | |
20.0 °C | 210.0 MPa Show Material materials with Zugfestigkeit of 210.0 MPa | H112 | EN 573-3 | Flat |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube | Long | |
150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 180.0 W/(m·K) | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 25000000.0 S/m | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
spezifischer Widerstand | 4e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 5e-08 Ω·m | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H112 | EN 573-3 | Profile, Rod, Sheet, Flat, Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H112 | EN 573-3, EN 485, EN 755 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Mangan | 0.5 - 1.1 % Show Material materials with Mangan of 0.5 - 1.1 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H112 | EN 573-3, EN 485, EN 755 | Profile, Rod, Sheet, Flat, Tube, Strip, Plate, Welded Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |