Allgemein
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Dichte | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
20.0 °C | 2.71 g/cm³ Show Material materials with Dichte of 2.71 g/cm³ | H15 | EN 573-3 | Tube |
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Dehnung | 2.0 % Show Material materials with Dehnung of 2.0 % | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A50 | |
3.0 % Show Material materials with Dehnung of 3.0 % | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | A100 | ||
20.0 °C | 2.0 % Show Material materials with Dehnung of 2.0 % | H15 | EN 573-3 | Tube | A50 | |
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | H15 | EN 573-3 | Tube | ||
Elastizitätsmodul | -270.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H15 | EN 573-3 | Tube | |
70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | H15 | EN 573-3 | Tube | ||
50.0 °C | 69.0 GPa Show Material materials with Elastizitätsmodul of 69.0 GPa | H15 | EN 573-3 | Tube | ||
100.0 °C | 68.0 GPa Show Material materials with Elastizitätsmodul of 68.0 GPa | H15 | EN 573-3 | Tube | ||
150.0 °C | 66.0 GPa Show Material materials with Elastizitätsmodul of 66.0 GPa | H15 | EN 573-3 | Tube | ||
200.0 °C | 63.0 GPa Show Material materials with Elastizitätsmodul of 63.0 GPa | H15 | EN 573-3 | Tube | ||
250.0 °C | 57.0 GPa Show Material materials with Elastizitätsmodul of 57.0 GPa | H15 | EN 573-3 | Tube | ||
300.0 °C | 50.0 GPa Show Material materials with Elastizitätsmodul of 50.0 GPa | H15 | EN 573-3 | Tube | ||
Härte, Brinell | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
20.0 °C | 80.0 [-] Show Material materials with Härte, Brinell of 80.0 [-] | H15 | EN 573-3 | Tube | ||
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 5000 Series Aluminium | ||||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 5000 Series Aluminium | ||||
Schubmodule | 20.0 °C | 26.5 Show Material materials with Schubmodule of 26.5 | H15 | EN 573-3 | Tube | |
Zugfestigkeit | 20.0 °C | 250.0 - 300.0 MPa Show Material materials with Zugfestigkeit of 250.0 - 300.0 MPa | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
100 °C | 2.3699999999999997e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.3699999999999997e-05 1/K | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Max. Betriebstemperatur | 150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | H15 | EN 573-3 | Tube | Long | |
150.0 °C Show Material materials with Max. Betriebstemperatur of 150.0 °C | Typical for Wrought 5000 Series Aluminium | |||||
Schmelzpunkt | 620.0 - 650.0 °C Show Material materials with Schmelzpunkt of 620.0 - 650.0 °C | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | ||
Spezifische Wärmekapazität | 879.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 879.0 - 963.0 J/(kg·K) | Typical for Wrought 5000 Series Aluminium | ||||
Wärmeleitfähigkeit | 20.0 °C | 140.0 - 180.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 140.0 - 180.0 W/(m·K) | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 20000000.0 - 25000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 20000000.0 - 25000000.0 S/m | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
spezifischer Widerstand | 4e-08 - 5e-08 Ω·m Show Material materials with spezifischer Widerstand of 4e-08 - 5e-08 Ω·m | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Chrom | 0.3 % Show Material materials with Chrom of 0.3 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Eisen | 0.5 % Show Material materials with Eisen of 0.5 % | H15 | EN 573-3 | Tube |
0.50 % Show Material materials with Eisen of 0.50 % | H15 | EN 573-3, EN 754 | Strip, Sheet, Plate, Rod, Tube, Welded Tube | |
Kupfer | 0.1 % Show Material materials with Kupfer of 0.1 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Magnesium | 1.6 - 2.5 % Show Material materials with Magnesium of 1.6 - 2.5 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Mangan | 0.5 - 1.1 % Show Material materials with Mangan of 0.5 - 1.1 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Titan | 0.1 % Show Material materials with Titan of 0.1 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Zink | 0.2 % Show Material materials with Zink of 0.2 % | H15 | EN 573-3, EN 754 | Tube, Strip, Sheet, Plate, Rod, Welded Tube |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: sufficient, Protective: good | |
Brazing | hard brazing (with flux/ without flux): poor / sufficient, friction soldering: acceptable, soft brazing with flux: poor | |
Corrosion properties | Seawater: very good, weathering: very good | |
Workability | Bending / Spinning (cold): good / acceptable, Impact extrusion (cold): sufficient, Deep drawing / upsetting (Condition) good (O) / good (H12) |