Allgemein
Mechanisch
Property | Temperature | Value | Condition | Related Standards | Shape | Comment |
---|---|---|---|---|---|---|
Bending Fatigue Strength | 60.0 - 90.0 MPa Show Material materials with Bending Fatigue Strength of 60.0 - 90.0 MPa | F | EN 1706, EN 13195 | Casting | ||
Dehnung | -196.0 °C | 11.4 % Show Material materials with Dehnung of 11.4 % | F | EN 1706 | ||
-120.0 °C | 10.9 % Show Material materials with Dehnung of 10.9 % | F | EN 1706 | |||
-50.0 °C | 10.9 % Show Material materials with Dehnung of 10.9 % | F | EN 1706 | |||
3.0 % Show Material materials with Dehnung of 3.0 % | F | EN 1706, EN 13195 | Casting | A50 | ||
5.0 % Show Material materials with Dehnung of 5.0 % | F | EN 1706, EN 13195 | Casting | A50 | ||
20.0 °C | 3.0 % Show Material materials with Dehnung of 3.0 % | F | EN 1706 | A50 | ||
20.0 °C | 7.6 % Show Material materials with Dehnung of 7.6 % | F | EN 1706 | |||
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | F | EN 1706 | |||
Härte, Brinell | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | F | EN 1706, EN 13195 | Casting | ||
20.0 °C | 50.0 [-] Show Material materials with Härte, Brinell of 50.0 [-] | F | EN 1706 | |||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Cast 5xx.x Series Aluminium | ||||
Zugfestigkeit | -196.0 °C | 213.0 MPa Show Material materials with Zugfestigkeit of 213.0 MPa | F | EN 1706 | ||
-120.0 °C | 188.0 MPa Show Material materials with Zugfestigkeit of 188.0 MPa | F | EN 1706 | |||
-50.0 °C | 170.0 MPa Show Material materials with Zugfestigkeit of 170.0 MPa | F | EN 1706 | |||
140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | F | EN 1706, EN 13195 | Casting | |||
150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706, EN 13195 | Casting | |||
20.0 °C | 140.0 MPa Show Material materials with Zugfestigkeit of 140.0 MPa | F | EN 1706 | |||
20.0 °C | 150.0 MPa Show Material materials with Zugfestigkeit of 150.0 MPa | F | EN 1706 |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting |
100.0 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting | |
100 °C | 2.4e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.4e-05 1/K | F | EN 1706, EN 13195 | Casting | |
Schmelzpunkt | 600.0 - 650.0 °C Show Material materials with Schmelzpunkt of 600.0 - 650.0 °C | F | EN 1706, EN 13195 | Casting | |
Spezifische Wärmekapazität | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | EN 1706, EN 13195 | Casting | |
20.0 °C | 940.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 940.0 J/(kg·K) | F | EN 1706 | ||
Wärmeleitfähigkeit | 20.0 °C | 130.0 - 140.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 130.0 - 140.0 W/(m·K) | F | EN 1706, EN 13195 | Casting |
Elektrisch
Property | Temperature | Value | Condition | Related Standards | Shape |
---|---|---|---|---|---|
Elektrische Leitfähigkeit | 20.0 °C | 17000000.0 - 22000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 17000000.0 - 22000000.0 S/m | F | EN 1706, EN 13195 | Casting |
spezifischer Widerstand | 4.55e-08 - 5.88e-08 Ω·m Show Material materials with spezifischer Widerstand of 4.55e-08 - 5.88e-08 Ω·m | F | EN 1706, EN 13195 | Casting |
Chemical properties
Property | Value | Condition | Related Standards | Shape |
---|---|---|---|---|
Aluminium | 94.45 % Show Material materials with Aluminium of 94.45 % | F | EN 1706 | |
Eisen | 0.55 % Show Material materials with Eisen of 0.55 % | F | EN 1706 | |
0.55 % Show Material materials with Eisen of 0.55 % | F | EN 1706, EN 13195 | Casting | |
Kupfer | 0.05 % Show Material materials with Kupfer of 0.05 % | F | EN 1706, EN 13195 | Casting |
Magnesium | 2.5 - 3.5 % Show Material materials with Magnesium of 2.5 - 3.5 % | F | EN 1706, EN 13195 | Casting |
Mangan | 0.45 % Show Material materials with Mangan of 0.45 % | F | EN 1706, EN 13195 | Casting |
Silizium | 0.55 % Show Material materials with Silizium of 0.55 % | F | EN 1706, EN 13195 | Casting |
Titan | 0.2 % Show Material materials with Titan of 0.2 % | F | EN 1706, EN 13195 | Casting |
Zink | 0.1 % Show Material materials with Zink of 0.1 % | F | EN 1706, EN 13195 | Casting |
Technological properties
Property | ||
---|---|---|
Anodizing | decorative: excellent | |
Corrosion properties | general: excellent | |
General machinability | after thermal treatment: excellent | |
Processing methods | permanent mould casting |