Allgemein
Property | Value | Condition | Related Standards |
---|---|---|---|
Dichte | 2.83 g/cm³ Show Material materials with Dichte of 2.83 g/cm³ | T3 | AA Standards, ASTM B210, ASTM B211 |
Mechanisch
Property | Value | Condition | Related Standards | Comment |
---|---|---|---|---|
Bending Fatigue Strength | 125.0 MPa Show Material materials with Bending Fatigue Strength of 125.0 MPa | T3 | AA Standards | |
Elastizitätsmodul | 70.0 GPa Show Material materials with Elastizitätsmodul of 70.0 GPa | T3 | AA Standards, ASTM B210, ASTM B211 | |
Härte, Brinell | 95.0 [-] Show Material materials with Härte, Brinell of 95.0 [-] | T3 | AA Standards | |
Plane-Strain Fracture Toughnes | 22.0 - 35.0 MPa·√m Show Material materials with Plane-Strain Fracture Toughnes of 22.0 - 35.0 MPa·√m | Typical for Wrought 2000 Series Aluminium | ||
Poissonzahl | 0.33 [-] Show Material materials with Poissonzahl of 0.33 [-] | Typical for Wrought 2000 Series Aluminium | ||
Schubmodule | 26.0 - 27.5 GPa Show Material materials with Schubmodule of 26.0 - 27.5 GPa | Typical for Wrought 2000 Series Aluminium | ||
Zugfestigkeit | 290.0 MPa Show Material materials with Zugfestigkeit of 290.0 MPa | T3 | AA Standards, ASTM B211 | |
295.0 MPa Show Material materials with Zugfestigkeit of 295.0 MPa | T3 | AA Standards, ASTM B211 | ||
310.0 MPa Show Material materials with Zugfestigkeit of 310.0 MPa | T3 | AA Standards, ASTM B211 | ||
325.0 MPa Show Material materials with Zugfestigkeit of 325.0 MPa | T3 | AA Standards, ASTM B210 | ||
380.0 MPa Show Material materials with Zugfestigkeit of 380.0 MPa | T3 | AA Standards |
Thermisch
Property | Temperature | Value | Condition | Related Standards | Comment |
---|---|---|---|---|---|
Koeffizient der thermischen Ausdehnung | 20 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | T3 | AA Standards, ASTM B210, ASTM B211 | |
100 °C | 2.2899999999999998e-05 1/K Show Material materials with Koeffizient der thermischen Ausdehnung of 2.2899999999999998e-05 1/K | T3 | AA Standards, ASTM B210, ASTM B211 | ||
Schmelzpunkt | 540.0 - 645.0 °C Show Material materials with Schmelzpunkt of 540.0 - 645.0 °C | T3 | AA Standards, ASTM B210, ASTM B211 | ||
Spezifische Wärmekapazität | 816.0 - 963.0 J/(kg·K) Show Material materials with Spezifische Wärmekapazität of 816.0 - 963.0 J/(kg·K) | Typical for Wrought 2000 Series Aluminium | |||
Wärmeleitfähigkeit | 151.0 - 172.0 W/(m·K) Show Material materials with Wärmeleitfähigkeit of 151.0 - 172.0 W/(m·K) | T3 | AA Standards, ASTM B210, ASTM B211 |
Elektrisch
Property | Value | Condition | Related Standards |
---|---|---|---|
Elektrische Leitfähigkeit | 23000000.0 - 26000000.0 S/m Show Material materials with Elektrische Leitfähigkeit of 23000000.0 - 26000000.0 S/m | T3 | AA Standards, ASTM B210, ASTM B211 |
spezifischer Widerstand | 3.85e-08 - 4.35e-08 Ω·m Show Material materials with spezifischer Widerstand of 3.85e-08 - 4.35e-08 Ω·m | T3 | AA Standards, ASTM B210, ASTM B211 |
Chemical properties
Property | Value | Condition | Related Standards |
---|---|---|---|
Bismut | 0.2 - 0.6 % Show Material materials with Bismut of 0.2 - 0.6 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Blei | 0.2 - 0.6 % Show Material materials with Blei of 0.2 - 0.6 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Eisen | 0.70 % Show Material materials with Eisen of 0.70 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Kupfer | 5.0 - 6.0 % Show Material materials with Kupfer of 5.0 - 6.0 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Silizium | 0.4 % Show Material materials with Silizium of 0.4 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Zink | 0.3 % Show Material materials with Zink of 0.3 % | T3 | AA Standards, ASTM B210, ASTM B211 |
Technological properties
Property | ||
---|---|---|
Brazing | general: no brazing is known or developed | |
Corrosion properties | Stress corrosion cracking: Limited operational damage(T3, T4, T451), no damage during operation, limited damage during laboratory tests (T8), general: sufficient, in principle it should be protected | |
General machinability | General: very good | |
Workability | general (condition): poor(T3), acceptable (T4, T451), d (T8) |